ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe

Share:

ISO 9080 Thermoplastic Pipe Long-Term Hydrostatic Strength Tester | UnitedTest

UnitedTest manufactures ISO 9080 compliant hydrostatic testing machines for thermoplastic pipes. Support the standard extrapolation method (SEM) to predict long-term hydrostatic strength without decades-long real-time ageing tests for plastic piping laboratories.


ISO 9080 Plastics piping and ducting systems defines the standard extrapolation method (SEM), a statistical extrapolation procedure used to predict the long‑term hydrostatic performance of thermoplastic pipe materials. This test method eliminates the need for multi‑decade real‑time ageing tests and delivers reliable long-term strength data for pipe design and pressure rating validation. UnitedTest provides integrated hydrostatic test systems tailored to ISO 9080 requirements for plastic pipe factories and third-party testing institutes.


According to ISO 9080, the longest static hydraulic test for pipes shall last for at least 9000 hours. The circumferential stress and failure time data at the time of pipe failure shall be classified using multiple linear regression method, and the MRS value of the material shall be determined based on the 97.5% confidence lower limit of the long-term static hydraulic strength for 50 years (438 000 hours). In the ASTM D2837 standard, the longest static hydraulic test for pipes should last at least 10000 hours, extrapolated to obtain an average long-term static hydraulic strength of 100000 hours (approximately 11.4 years), classified to determine the HDB value. According to ASTM D2837, each temperature should be evaluated independently, so there is no temperature variable in its linear regression model. In ISO 9080, low-temperature data can be extrapolated from high-temperature test results.


ISO 9080 Hydrostatic Pressure Testing Machine for pipe sample:
ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe testing
Advanced Hydrostatic Pressure Testing Service/Equipment


Test Principle

The core principle is multiple linear regression analysis based on log₁₀‑stress versus log₁₀‑time stress‑rupture data collected at multiple elevated test temperatures.

  1. Pipe specimens are subjected to constant internal hydrostatic pressure at different temperatures, recording hoop stress and failure‑to‑leak time.

  2. The model uses 2‑, 3‑ or 4‑parameter mathematical formulas (Annex A) to fit stress‑rupture data, converting short‑term laboratory failure data into long‑term performance predictions.

  3. It calculates LTHS (Long‑Term Hydrostatic Strength, predicted mean strength) and LPL (97.5% lower prediction limit). LPL is the critical design value representing the 97.5% one‑sided lower statistical bound of predicted failure stress.

  4. The standard defines the “knee” phenomenon: a transition point between two failure modes (type A high‑stress ductile failure, type B low‑stress brittle failure) on log‑log stress‑time curves. Annex B provides automatic knee‑detection algorithms via F‑test statistics; datasets are split and regressed separately if a statistically significant knee exists.

  5. Extrapolation time factor ke limits valid extrapolation ranges, based on Arrhenius temperature‑dependence behaviour for polyolefins and vinyl‑chloride‑based polymers, to avoid over‑extrapolation beyond reliable data boundaries.


Test Specimen Information

Dimensions: Same nominal dimension for all test specimens; mean outer diameter and minimum wall thickness are measured following ISO 3126 to calculate hoop stress from internal pressure.

Material requirements: Specimens shall come from the same material batch and production run. For legacy materials evaluated by older ISO 9080 editions, supplementary data from other batches are permitted if evenly distributed across test temperatures and documented in test reports.


Test Equipment required for the ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe

Pipe Hydrostatic Pressure Test System

Complies with ISO 1167‑1 and ISO 1167‑2, to apply constant internal hydrostatic pressure to pipe samples, maintain stable test temperature, record leak‑failure time of each specimen. 

Water is the preferred internal pressurizing medium which must not chemically degrade pipe material.

Enclosures

End caps, Type A.

Supports/hangers — keep specimens apart and off tank walls.

Temperature‑controlled bath & circulating pump

Thermostatically controlled hot‑water bath to circulate test fluid and stabilize specimen temperature within ±5 °F (±3 °C). 

Fluid circulates during pressure‑off periods of each cycle.

Thermal analysis instruments

Vicat softening temperature tester (ISO 2507‑1), for amorphous glassy polymers to set maximum permissible test temperature.

DSC differential scanning calorimeter (ISO 11357‑3), for semi‑crystalline polymers to measure melting temperature for upper test‑temperature limits.


Test Parameters:

Test temperature T_t: Controlled test temperature (converted to Kelvin for regression formulas). At minimum one test temperature shall be 20 °C or 23 °C; adjacent test temperatures differ 10 °C ~ 50 °C. Maximum test temperature is limited to 15 °C below Vicat (amorphous PVC‑based) or melting point (semi‑crystalline polyolefin).

Time‑to‑failure: Hours until pipe leak occurs; test data with failure time ≤10 h shall be discarded; ≤1000 h may be discarded for ≤40 °C if dataset size requirements are satisfied.


General Test Procedures of ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe

  1. Specimen preparation: Fabricate pipe test pieces per ISO 1167‑2; measure outer diameter and minimum wall thickness following ISO 3126.

  2. Stress‑rupture testing: Perform constant‑internal‑pressure tests according to ISO 1167‑1 at ≥2 different temperatures (one being 20 °C / 23 °C, temperature spacing 10‑50 °C). Record test temperature, applied pressure, failure time, failure mode (ductile/brittle). Collect sufficient long‑time failure points (>7000 h, >9000 h). Discard failure data below 10 h; optionally discard points ≤1000 h for ≤40 °C if data quantity meets requirements.

  3. Pre‑process dataset: Remove failures caused by contamination; keep censored non‑failed specimens as allowed.

  4. Knee detection: Apply Annex‑B automatic knee‑detection F‑test for each test temperature. If a statistically significant knee is confirmed, split dataset into type‑A (high‑stress) and type‑B (low‑stress) subsets. Perform manual re‑classification if automatic output conflicts with visual log‑log plot, document all justifications.

  5. Statistical regression: Run multiple‑linear regression (Annex A) separately for type‑A and type‑B datasets, select appropriate 2‑/3‑/4‑parameter model, execute goodness‑of‑fit F‑test.

  6. Calculate extrapolation boundaries: Compute t_max from five longest failure times, apply material‑specific k_e factors to calculate allowable extrapolation time t_e. Predict LTHS and 97.5% LPL for target time‑temperature conditions (e.g. 20 °C for 50 years) within permitted extrapolation limits.

  7. Visual verification: Plot raw data points, regression lines for LTHS and LPL curves on log₁₀‑stress vs log₁₀‑time chart.

  8. Compile test report: Include standard reference, material batch information, pipe dimensions, test medium, full observation table, discarded‑point information, knee‑classification notes, model parameters, residual statistics, plotted graph, software information and test anomalies as required by ISO 9080.

ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe testing

Related Standards: 

ASTM D2143

Standard Test Method for Cyclic Pressure Strength of Reinforced, Thermosetting Plastic Pipe

ASTM D2992Practice for Obtaining Hydrostatic or Pressure Design Basis for Fiberglass (Glass-Fiber-Reinforced Thermosetting-Resin) Pipe and Fittings
ASTM D1598Time-to-failure under constant internal pressure (Procedure B)
ASTM D1599short-time hydraulic pressure (used to verify scaling of fittings/joints)
ISO 1167Thermoplastics pipes, fittings and assemblies for the conveyance of fluids - Determination of the resistance to internal pressure
AWWA C950fiberglass pressure pipe (US water-works practice)
ISO 14692 Petroleum and natural gas industries - Glass-reinforced plastics (GRP) piping
ISO 9080Plastics piping and ducting systems - Determination of the long-term hydrostatic strength of thermoplastics materials in pipe form by extrapolation
ASTM D2837Obtains HDB/PDB for thermoplastic plastic pipe (similar statistical logic but for non‑reinforced thermoplastics, not fiberglass thermoset composites)


Industry fields of application

  • Material classification — the resin producer's route to an MRS rating (PE 63 / PE 80 / PE 100, PP‑H/PP‑B/PP‑R grades, PB, PVC‑U, PE‑X, PVDF…). ISO 9080 classification is normally certified by the compound producer, and the rating travels with the compound .

  • Pressure pipe design — converts to design stress via the service coefficient C (σ_design = MRS / C), feeding wall‑thickness/SDR and pressure‑class calculations.

  • Sectors — potable water and gas distribution (PE), hot & cold water plumbing and underfloor heating (PP‑R, PE‑X, PB), sewerage and drainage, industrial fluid/chemical conveyance (PVDF, PVC‑C), district heating and cooling, mining and irrigation.

  • Users — raw‑material producers (grade development and datasheets), pipe extruders (qualification), independent test laboratories, certification bodies, specifiers and asset owners.

  • Product‑standard gatekeeping — many product standards add criteria on top of ISO 9080, e.g. PE 100 requires that no knee appears on the 80 °C curve before a specified time; a resin that "knees" early cannot reach PE 100 regardless of short‑term performance .


Keywords: ISO 9080 tester, thermoplastic pipe hydrostatic strength test machine, long term hydrostatic strength tester, SEM extrapolation pipe test rig, plastic pipe hydrostatic pressure tester, pipe rupture test equipment, HDPE pipe long-term hydrostatic test, PP pipe hydrostatic ageing test, plastic piping system lab testing, ISO 9080 hydrostatic test fixture, thermoplastic pipe pressure life extrapolation tester, pipe material long-term strength verification machine

Related products and device

ISO 9080 Long Term Hydrostatic Pressure Testing Machine for Thermoplastic Pipe

hydrostatic pressure testing machine is designed according to ISO 1167, ASTM D1598, ASTM D1599. Under a stipulated constant hydrostatic pressure force, keeping provision time; or inside the pipe, apply a constant and rapid hydraulic pressure to make the specimen broken in a short period time, check the max. pressure force, then calculate the ring stress.

ISO 9080 plastic pipe hydrostatic pressure tester constant temperature tank

Constant temperature water tank is a crucial piece of equipment for hydrostatic pressure tests, particularly for long-term and burst tests. It is designed to maintain a constant pressure and temperature during testing, which is essential for accurately assessing the strength and durability of pipe.

ISO 9080 End cap of pipe pressure test

Stainless Steel End Caps For Pipe Hydrostatic Pressure and Burst Testing are designed for internal hydrostatic pressure testing of pipes and fittings. It is used to seal the sample in order to generate internal pressure in the sample, with the characters: ISO 1167 Type A structure.

Related Standard

ISO 1167 Thermoplastics pipes resistance to internal pressure test –

ISO 1167: 2006 Thermoplastics pipes, fittings and assemblies for the conveyance of fluids -- Determination of the resistance to internal pressure.

ISO 1167 test method specifies a general test method for determining the resistance to internal hydrostatic pressure at a given temperature of thermoplastics pipes, fittings and piping systems for the transport of fluids. The method accommodates water-in-water, water-in-air and water-in-liquid tests. It defines uniform hydrostatic pressure testing to evaluate short-term and long-term pressure-bearing durability of thermoplastic fluid-transport piping systems.


Hydrostatic pressure testing is a valuable method for assessing the strength and integrity of pressurized systems, ensuring that they can meet operational demands without failure. Hydrostatic pressure testing can evaluate these items by filling pipelines, tanks, or containers with water before pressure is applied to detect any potential leaks or issues. 

Hydrostatic pressure tester is critical across multiple industries, from pipeline engineering to industrial piping. It helps prevent costly failures or leaks by verifying whether the system can safely reach the specified pressure levels.

ASTM D1598 test for long-term hydrostatic pressure of plastic pipe –

ASTM D1598 Standard Test Method for Time-to-Failure of Plastic Pipe Under Constant Internal Pressure. It is a fundamental test method used to determine the long-term hydrostatic strength and resistance of thermoplastic pipe by applying a constant internal pressure until the pipe specimen fails (ruptures). Which is critical for establishing hydrostatic design basis and ensuring long-term pipeline reliability.

ASTM D2241 PVC SDR Pressure Rated Pipe Testing Methods –

ASTM D2241 Standard Specification for Poly(Vinyl Chloride) (PVC) Pressure-Rated Pipe (SDR Series)

ASTM D2241 governs SDR‑series PVC pressure pipes for pressurized water and chemically‑compatible pressurized liquids. The mechanical performance test include sustained pressure, burst pressure, flattening, extrusion quality and impact, plus marking rules.


ASTM D2143 Cyclic Pressure Test for Reinforced Thermosetting Plastic Pipe –

ASTM D2143 Standard Test Method for Cyclic Pressure Strength of Reinforced, Thermosetting Plastic Pipe

ASTM D2143 determines the failure characteristics of reinforced thermosetting plastic pipe under cyclic internal hydraulic pressure — i.e., how many pressure cycles a pipe survives at a given pressure/stress level. Its real purpose is not to pass/fail a single pipe, but to generate the stress‑vs‑cycles‑to‑failure data points that feed the regression analysis in ASTM D2992 Procedure A, from which the long‑term Hydrostatic Design Basis (HDB) and pressure rating of a pipe product are derived.


ASTM D2992 Fiberglass Pipe Hydrostatic Test for Obtaining Hydrostatic or Pressure Design Basis –

ASTM D2992 Practice for Obtaining Hydrostatic or Pressure Design Basis for Fiberglass (Glass-Fiber-Reinforced Thermosetting-Resin) Pipe and Fittings

ASTM D2992 is not a "pass/fail" test — it is a statistical extrapolation practice. It defines how to take short-term pressure-rupture data on fiberglass (GRP) pipe and fittings, fit a log-log regression line, and extrapolate it to a 50-year design life in order to publish a Hydrostatic Design Basis (HDB) or Pressure Design Basis (PDB) for that specific product and manufacturing process.

EN 1796 GRP-UP Pipe Mechanical & Pressure Test Methods –

EN 1796 Plastics piping systems for water supply with or without pressure — Glass‑reinforced thermosetting plastics (GRP) based on unsaturated polyester resin (UP)

EN 1796 is the European product/system standard for plastics piping systems for water supply with or without pressure, made from glass-reinforced thermosetting plastics (GRP) based on unsaturated polyester (UP) resin. It covers pipes, fittings (bends, branches, reducers, saddles, flanged adaptors) and joints, classifies them by DN / PN / SN, and sets the type-test (TT) and batch-release (quality-control) test scheme that a manufacturer, a certification body or a third-party laboratory must run to prove a 50-year design life for buried (and, with care, non-buried) water pipelines.

It defines material composition (E‑glass/C‑glass/R‑glass reinforcement, UP resin, elastomer gaskets), wall‑layer construction (inner liner, structural layer, outer protective layer), dimensional tolerances, marking rules, mechanical performance, long‑term creep, hydrostatic pressure resistance and full joint performance requirements. 


ISO 13254 Plastic pipe and joints watertightness test by internal hydrostatic pressure –

ISO 13254 specifies a hydrostatic pressure test method for evaluating the watertightness of two categories of non-pressure thermoplastics components: (1) multi-piece fabricated products (e.g., custom-molded fittings) and (2) joints in thermoplastics piping systems.The test validates sealing performance under simulated service conditions for drainage, sewerage, and stormwater systems.

The standard aims to ensure consistent assessment of leak resistance, critical for applications like drainage, irrigation, and underground conduits where fluid ingress could compromise system integrity.

ISO 4437-1 Tensile, Hydrostatic pressure test for Plastics PE piping systems for the supply of gaseous fuels –

ISO 4437-1:2024 Plastics piping systems for the supply of gaseous fuels — Polyethylene (PE) Part 1: General

ISO 4437-1:2014 specifies the general properties of polyethylene (PE) compounds for the manufacture of pipes and fittings intended to be used for the supply of gaseous fuels. It also specifies the test parameters for the test methods referred to in this International Standard.   

ASTM D1598, D1599 Plastic Pipe Constant or short time pressure testing methods –

ASTM D1598: Standard Test Method for Time-to-Failure of Plastic Pipe Under Constant Internal Pressure.

ASTM D1598 test method covers the determination of the time-to-failure of both thermoplastic and reinforced thermosetting/resin pipe under constant internal pressure.This test method provides a method of characterizing plastics in the form of pipe under the conditions prescribed.


ASTM D1599: Standard Test Method for Resistance to Short-Time Hydraulic Pressure of Plastic Pipe, Tubing, and Fittings.

ASTM D1599 test method establishes the short-time hydraulic failure pressure of thermoplastic or reinforced thermosetting resin pipe, tubing, or fittings. Data obtained by this test method are of use only in predicting the behavior of pipe, tubing, and fittings under conditions of temperature, time, method of loading, and hoop stress similar to those used in the actual test. They are generally not indicative of the long-term strength of thermoplastic or reinforced thermosetting resin pipe, tubing, and fittings


ASTM D1599 Pipe short-time hydraulic burst pressure test –

ASTM D1599 is titled "Standard Test Method for Resistance to Short-Time Hydraulic Pressure of Plastic Pipe, Tubing, and Fittings." It is a fundamental short-term, destructive pressure test used to determine the ultimate failure pressure (often called the "burst pressure") of thermoplastic pipe, tubing, or fittings under rapidly applied internal pressure at a specified temperature. Typically completed within 60–70 seconds, mainly for quality control and short-term design validation. 

Frequently Asked Questions: ISO 9080 Long Term Hydrostatic Pressure Test for Thermoplastic Pipe

1, What is ISO 9080?

ISO 9080:2012 is the International Standard that specifies a method for predicting the long-term hydrostatic strength of thermoplastics materials in pipe form by statistical extrapolation. It was developed from pipe stress-rupture data and applies to all types of thermoplastics pipe at applicable temperatures. It was prepared by ISO/TC 138/SC 5, published in October 2012 (2nd edition) and confirmed again in 2023, so it remains the current edition.


2, Is ISO 9080 a test method or a calculation method?

Strictly, it is a method of analysis, but in industry it is used as a complete test programme. The physical work — pressurising pipe sections until they leak — is carried out per ISO 1167-1/ISO 1167-2. ISO 9080 then takes those stress-rupture points and performs the Standard Extrapolation Method (SEM): multiple linear regression in log(stress) vs log(time) space with temperature as a second variable, producing a predicted strength surface and its statistical limits.


3, Why is ISO 9080 so important?

Because nobody can wait 50 years to qualify a pipe material. ISO 9080 is the statistically defensible bridge from roughly one year of measured data (points beyond 9 000 h are required) to a 50-year design value. It defines the 97.5 % lower prediction limit (LPL), which after categorisation in ISO 12162 becomes the MRS — the number behind PE 80, PE 100, PP-R and similar grade designations, and the basis for allowable pressure and wall-thickness design worldwide.


4, What is the difference between ISO 9080 and ISO 1167?

ISO 1167 (Parts 1 and 2) is the laboratory pressure test: apparatus, end caps, temperature control, procedure, specimen preparation. ISO 9080 is what you do with the resulting data: the regression, knee detection, extrapolation limits and confidence limits. In practice a laboratory runs ISO 1167 to generate data and ISO 9080 to analyse it, and ISO 9080 makes ISO 1167-1/2 normative.


5, What kind of test specimen is required?

The material must be tested in pipe form — complete straight pipe sections, not machined coupons. All pipes feeding one analysis must have the same nominal dimensions and come from the same batch of material and the same production run. For materials already evaluated under ISO/TR 9080:1992 or ISO 9080:2003, the original data set may be complemented with additional batches, spread regularly over each temperature and documented in the report.


6, What are the dimensional requirements for a test piece?

Per ISO 1167-2, the free length between end caps must be at least three times the nominal outside diameter, with a minimum of 250 mm; for pipes above 315 mm outside diameter the free length may be reduced to twice the diameter if agreed in the referring standard. Mean outside diameter and minimum wall thickness are measured to ISO 3126 and used to convert test pressure into hoop stress. Injection-moulded tubular test pieces (25–110 mm diameter) are permitted for injection-moulding materials and their results can also be extrapolated by ISO 9080.


7, What equipment is needed?

A constant-temperature environment (water bath held to ±1 °C, or air oven held to −1/+2 °C), pressurising equipment able to hold pressure within −1 %/+2 % for the whole test, Type A end caps, supports/hangers, calibrated pressure and temperature measuring devices, timers, ISO 3126 dimensional equipment — all per ISO 1167-1 — plus SEM software implementing ISO 9080 Annex A (regression models) and Annex B (automatic knee detection).


8, Why does ISO 9080 require Type A end caps?

Type A end caps are rigidly fixed to the test piece and transmit the hydrostatic end thrust into the pipe wall, so the specimen is under the true biaxial (hoop plus axial) stress state. Type B caps are connected to each other and absorb the end thrust, giving a different stress state and different times to failure. ISO 1167-1 states explicitly that Type A caps shall be used when determining long-term hydrostatic strength in accordance with ISO 9080.


9, What should a laboratory look for in a testing machine for this work?

Station capacity to hold the full matrix in parallel (typically 60–150+ stations running for a year or more), per-station pressure regulation so one failure cannot disturb the others, bath temperature stability of ±1 °C verified across the working volume, automatic leak/failure detection that stops the individual timer, continuous data logging, and an export of stress, time, temperature and failure mode per station that drops straight into ISO 9080 analysis software.


10, Which temperatures must be used?

Two or more temperatures, with adjacent temperatures separated by at least 10 °C and at most 50 °C. One temperature must be 20 °C or 23 °C. The highest test temperature must not exceed the Vicat softening temperature (ISO 2507-1) minus 15 °C for glassy amorphous polymers, or the DSC melting temperature (ISO 11357-3) minus 15 °C for semi-crystalline polymers. The range should bracket the intended service temperature.


11, How long does an ISO 9080 programme take?

The regression requires times of 9 000 h or longer, so in practice the data-collection phase runs for at least 12–18 months. The analysis itself (knee detection, regression, LPL calculation, extrapolation check) is then a matter of minutes with suitable software.


12, What is the 'knee' and why does it matter?

The knee is the point where the log(stress)–log(time) curve bends: the transition from one failure mechanism to another — in polyolefins typically from ductile failure to quasi-brittle slow crack growth. Points above the knee are data type A, points below are data type B, and the two branches are fitted independently. Detecting the knee correctly is what separates a material that only looks good in short-term tests from one that genuinely performs at 50 years; product standards such as ISO 4427 use knee behaviour as a disqualifying criterion for the highest grade.


12, What is the difference between LPL and LCL?

LPL is the lower prediction limit for an individual predicted value; LCL is the lower confidence limit for the mean strength. Several ISO documents incorrectly label the LPL as an LCL — ISO 9080 flags this explicitly in a footnote. For design and classification, the LPL is the correct, conservative quantity.


13, How do MRS and CRS relate to ISO 9080?

ISO 12162 takes the σ_LPL value and rounds it down to the next lower step of a preferred-number series. Categorised at 20 °C and 50 years it is called MRS (Minimum Required Strength) and is used to classify the material. Categorised at another design time or temperature it is called CRS_θ and is used directly for design. Design stress is then obtained by applying the overall service coefficient C.


14, Which industries rely on ISO 9080?

Potable water and gas distribution (PE), hot and cold water plumbing and underfloor heating (PP-R, PE-X, PB), drainage and sewerage, district heating and cooling, irrigation and mining, and industrial chemical conveyance (PVDF, PVC-C). Users include resin producers qualifying a new grade, pipe extruders, independent test laboratories, certification bodies, specifiers and asset owners.


15, How does ISO 9080 compare with ASTM D 2837?

Both analyse the same kind of stress-rupture data, but ASTM D 2837 determines the Hydrostatic Design Basis (HDB) from the mean long-term hydrostatic strength at 100 000 h, typically at 23 °C, regressing each temperature individually with a two-coefficient equation and assuming linearity. ISO 9080 combines all temperatures in one regression, uses the 97.5 % LPL rather than the mean, targets 50 years at 20 °C, and explicitly models a knee with 2-, 3- or 4-parameter models. Actual long-term performance of a given material is the same under the same conditions; only the statistical basis differs.


16, Why choose ISO 9080 long-term hydrostatic strength testing machine from UnitedTest? 

UnitedTest is professional manufacturer of ISO 1167 hydrostatic pressure test equipment supporting ISO 9080 long-term hydrostatic strength extrapolation for PE, PP, PVC pressure pipes. Our multi-station pipe hydrostatic testers provide stable constant pressure & temperature testing for ISO 9080 LPL, MRS and 50-year life prediction for plastic piping labs and pipe factories.


UnitedTest designs and manufactures high-performance hydrostatic pressure test systems specially built to support ISO 9080 projects for plastic pipe manufacturers, third-party certification laboratories, R&D institutes and material testing centres worldwide. Our multi-station hydrostatic pipe testers deliver precise constant pressure control, independent temperature baths, long-duration unattended running and automatic failure logging, fully complying with ISO 1167‑1 and ISO 1167‑2. Test data exported from UnitedTest machines can be directly imported into validated ISO 9080 Standard Extrapolation Method software for knee detection, regression analysis, LPL calculation and MRS classification according to ISO 12162.


We support testing of PE, PP, PVC-U, PVC-C, PVDF pressure pipes used in drinking water supply, natural gas distribution and industrial fluid transport. UnitedTest provides one-stop pipe testing solutions including hydrostatic testers, burst testers, ring stiffness machines and related technical guidance for ISO 9080 testing workflow. If you need reliable test equipment to run ISO 9080 long-term hydrostatic strength qualification, contact UnitedTest for custom configuration and quotation.

< Previous: ISO 8645 Mopeds Light-alloy wheels testing

> Next: ISO 9237 Textiles Determination the permeability of fabrics to air

Require More Customized Solutions?

We offer customization to meet your specific needs. Our expert team will collaborate with you to develop the perfect product for you