ISO 899-2 Flexural Creep Tester | Three-Point Loading Plastic Creep Test Machine - UnitedTest
UnitedTest manufactures ISO 899-2 flexural creep testing machines for measuring time-dependent bending deformation of rigid, semi-rigid, filled and fibre-reinforced plastics under stable temperature and humidity conditions. Our three-point loading creep test equipment delivers reliable long-term flexural creep data for plastic material R&D, quality control and engineering design validation.
ISO 899-2 Plastics — Determination of creep behaviour — Part 2: Flexural creep by three-point loading
ISO 899-2 specifies a standardized laboratory method to measure the time-dependent bending deformation of a freely supported plastic beam under constant mid-span load, with strictly controlled pre-treatment, temperature and humidity environments. This flexural creep test evaluates how plastic specimens deform continuously over extended periods under sustained bending stress, which is critical for predicting long-term service performance of plastic components. It applies to rigid and semi-rigid, non-reinforced, filled and fibre-reinforced plastics, covering specimens directly moulded or machined from plastic sheets and finished moulded articles. UnitedTest supplies professional ISO 899-2 three-point flexural creep testing machines, supporting stable long-duration loading, precise displacement monitoring and environmental condition control to meet the standard’s requirements for polymer material testing, product qualification and technical data documentation.
Test Principle:
This standard defines a method to characterize the time-dependent flexural deformation of plastics using a simply supported beam loaded at mid-span (three-point bending configuration).
Core definition of creep: The increase in specimen strain over time under a constant applied force, measured starting from the moment full load is applied.
Working mechanism: A constant static force is applied at the center of the specimen, and mid-span deflection is recorded at predefined time intervals. From deflection data, key viscoelastic properties are derived to describe how the material deforms under sustained bending load.
The test quantifies the viscoelastic nature of polymers, where deformation is not instantaneous but evolves with time under constant stress.

Test Specimen Information:
Preferred specimen
The standard recommends a rectangular bar with the following dimensions:
Length: 80 ± 2 mm
Width: 10.0 ± 0.2 mm
Thickness: 4.0 ± 0.2 mm
Alternative specimens
When the preferred geometry is not feasible, specimen width is scaled to nominal thickness:
| Nominal thickness range (mm) | Standard width (mm, ±0.5) |
|---|---|
| 1 < h ≤ 3 | 25.0 |
| 3 < h ≤ 5 | 10.0 |
| 5 < h ≤ 10 | 15.0 |
| 10 < h ≤ 20 | 20.0 |
| 20 < h ≤ 35 | 35.0 |
| 35 < h ≤ 50 | 50.0 |
ISO 899-2 Plastic three-point flexural creep test Required Testing Equipment:
| Creep Test Machine | Rigid frame with two supports; levelled; enough clearance below the specimen for long-term flexure. Span adjustable to 16h for normal specimens; for rigid unidirectional-fibre-reinforced specimens, >17h or a fixed 100 mm span is allowed to avoid shear/compression-zone delamination. Applies load smoothly without transient overload; maintains the load within ±1 % of the desired load; allows rapid, smooth, reproducible loading; in creep-to-rupture tests, rupture shocks must not be transmitted to adjacent loading systems. |
| Loading edge and supports | loading-edge radius R1=5±0.1mm; support radius R2=2±0.2 mm for h>3 mm and R2=5±0.2 mm for h>3mm. |
| Deflection-measuring device | Contact or contactless; must not influence the specimen by mechanical effects (deformation, notches), physical effects (heating), or chemical effects. It shall conform to Class 1 of ISO 9513. At calibration, its initial position must correspond to its position at the unloaded specimen before the test. A deflectometer is required for engineering-design data; loading-edge/support displacement is permitted for research or QC. |
| Tools | Time-measurement device: accurate to 0.1%. Micrometer: resolution ≤ 0.01 mm, for specimen width and thickness. Vernier callipers: accurate to 0.1% of the span, for support distance measurement. Environmental chamber: maintains test temperature within ±2 °C and controlled humidity. |
Key Test Parameters:
Stress selection: Chosen to match the material’s intended application. Maximum deflection must never exceed 0.1 times the support span at any point during testing.
Temperature control: Temperature variation during testing must remain within ±2 °C.
Loading rate: Full load is applied progressively over 1–5 seconds, with a consistent rate across all tests in a series.
Deflection measurement schedule: Recommended time points include 1, 3, 6, 12, 30 minutes, followed by 1, 2, 5, 10, 20, 50, 100, 200, 500, 1000 hours, etc. More frequent readings are required if discontinuities in the creep curve are observed.
Time accuracy: Measured within ±0.1% or 2 seconds (whichever tolerance is less strict).
Optional recovery test: After non-rupture tests, the load is removed rapidly and deflection recovery is recorded using the same time schedule.
Test procedure of ISO 899-2 Plastic three-point flexural creep test
Specimen conditioning: Condition specimens under controlled temperature and humidity, with controlled thermal history (physical ageing strongly impacts creep behavior, as detailed in Annex A).
Dimensional and span measurement: Measure specimen width and thickness per ISO 16012 and ISO 178. Set the support span and verify it to within ±0.5% accuracy.
Specimen mounting: Place the conditioned specimen symmetrically on the supports, with its long axis perpendicular to the support edges. Position the deflection measurement system.
Stress and load calculation: Select the target flexural stress level and calculate the corresponding applied force.
Preloading (if required): Apply a small preload only after the specimen reaches test temperature and humidity. Zero the deflection device immediately after preloading. The preload counts toward the total test load.
Full loading: Apply the full test load smoothly over 1–5 seconds. Record the moment full load is reached as t = 0.
Deflection data collection: Record mid-span deflection at each scheduled time point.
Environmental monitoring: Record temperature and humidity at test start, at least three times per day initially, and at least once per day once conditions stabilize.
Optional recovery measurement: Remove the load rapidly at test conclusion and track deflection recovery over time.
Rupture testing (if applicable): Record the time to rupture if the specimen fails during testing.
Industries Application:
This test method serves three primary purposes:
Engineering design: Provides long-term deformation data for structural plastic components subjected to sustained bending loads (e.g. brackets, beams, panels, housings).
Quality control: Verifies batch-to-batch consistency of manufactured plastic materials.
Research and development: Evaluates new polymer formulations, filler systems, fibre reinforcements, and processing conditions.
It applies to rigid and semi-rigid plastics, including non-reinforced, filled, and short/long fibre-reinforced materials (both directly moulded and machined specimens).
It is not suitable for rigid cellular plastics (ISO 1209-1 and ISO 1209-2 cover those materials).
It may be unsuitable for some fibre-reinforced materials due to fibre orientation effects.
Common industries using this test include automotive, aerospace, construction, electrical/electronics, and industrial equipment manufacturing.
Related Test Standard
| ISO 178 | Plastics — Determination of flexural properties (the foundational standard for plastic bending testing, defining specimen geometry and bending fundamentals) |
| ASTM D695 | Test Method for Compressive Properties of Rigid Plastics (compressive specimen basis) |
| ASTM D790 | Test Methods for Flexural Properties (three-point bending method) |
| ASTM D6112 | compressive/flexural creep of plastic lumber and shapes |
| ISO 1209-1 | Flexural testing standards for rigid cellular plastics |
| GB/T 11546.2 | Plastics—Determination of creep behaviour—Part 2:Flexural creep by three-point loading |
| ISO 899-1 | Tensile creep and creep-rupture |
| ISO 899-2 | Flexural creep Test |
| ASTM D1780 | Practice for conducting creep tests of metal‑to‑metal adhesives, typically dead‑weight/lever tensile‑shear creep, temperature/time based. |
| ASTM D2990 | Standard Test Methods for Tensile, Compressive, and Flexural Creep and Creep-Rupture of Plastics |
The directly comparable international family — ASTM D2990 VS ISO 899
| ASTM D2990 | ISO 899-1 | ISO 899-2 | |
|---|---|---|---|
| Mode | Tensile + compressive + flexural (3-pt & 4-pt) in one document | Tensile creep (and creep to rupture) | Flexural creep by three-point loading only |
| Specimen | D638 Type I/II; D695; D790 bar | ISO 527-1A/1B dumb-bells, moulded or machined | 10 × 4 × 80 mm bar from the multipurpose specimen |
| Strain measurement | Direct on specimen preferred; grip separation permitted with correction factors; anvil displacement OK for compression | Extensometer on gauge length required for engineering-design data; grip separation only for research/QC | Die movement corrected for rig self-deformation, or optical/video |
| Compressive creep | Covered | No | No |
Keywords: ISO 899-2, flexural creep tester, three-point loading creep test machine, plastic creep testing equipment, polymer flexural creep, rigid plastic creep test, fibre reinforced plastic creep, filled plastic creep measurement, long term bending deformation test, plastic creep modulus, creep strain test, thermoplastic creep tester, thermoset plastic creep test, plastic material quality control, polymer engineering testing, creep test fixture, environmental controlled creep test, plastic beam creep test, UnitedTest creep machine, ISO 899-2 test equipment, plastic R&D creep testing, flexural creep rupture test, plastic long term performance test
Related products and device
Related Standard
ASTM D2990 Standard Test Methods for Tensile, Compressive, and Flexural Creep and Creep-Rupture of Plastics
ASTM D2990 defines procedures to measure time-dependent deformation (creep) and time-to-failure (creep-rupture) of plastic materials under constant static load and controlled environmental conditions.
ISO 899-1 Plastics — Determination of creep behaviour — Part 1: Tensile creep
ISO 899-1 determines tensile creep of plastics in the form of standard test specimens under specified conditions of pretreatment, temperature and humidity. It applies to rigid and semi-rigid, non-reinforced, filled and fibre-reinforced plastics, using dumb-bell-shaped specimens that are either directly moulded or machined from sheets or moulded articles.
ISO 527-1 covers the test procedures for determining tensile properties of plastics and plastic composites. Tensile properties of plastics that are determined through the practices of ISO 527-1 include tensile strength, tensile modulus and other properties related to stress strain characteristics of plastic materials.
ISO 527-2 specifies the test conditions for determining the tensile properties of moulding and extrusion plastics, based upon the general principles given in ISO 527-1. The methods described in ISO 527-2 are selectively suitable for use with the following range of materials: rigid and semi-rigid thermoplastics moulding, extrusion and cast materials, including compounds filled and reinforced by, for example, short fibres, small rods, plates or granules but excluding textile fibres (see ISO 527-4 and ISO 527-5).
ASTM D638 determining the tensile properties of unreinforced and reinforced plastics using dumbbell-shaped (dogbone) specimens tested under closely controlled conditions of conditioning, temperature, humidity, and crosshead speed. For measuring the tensile mechanical properties of unreinforced and reinforced plastics, including thermoplastics, thermosets, molded plastics, and plastic composites.
ASTM D695: Standard Test Method for Compressive Properties of Rigid Plastics
ASTM D695 test covers the determination of the mechanical properties of unreinforced and reinforced rigid plastics, including high-modulus composites, when loaded in compression at relatively low uniform rates of straining or loading. Test specimens of standard shape are employed. This procedure is applicable for a composite modulus up to and including 41,370 MPa (6,000,000 psi). It is technically equivalent to ISO 604 Plastics‑Determination of Compressive Properties. This test applies end‑loading compression on standard‑geometry specimens under controlled environmental and displacement‑rate conditions, delivering compressive strength, yield strength, offset yield strength, compressive elastic modulus, and compressive deformation data.
ASTM D790: Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials
ASTM D790 determines flexural (bending) properties for unreinforced plastics, reinforced plastics, high‑modulus composites and electrical insulating materials via three‑point bending on simply‑supported rectangular beam specimens. It applies to rigid and semi‑rigid materials. Flexural strength cannot be calculated if the specimen neither yields nor fractures on its outer surface before reaching 5 % maximum outer‑fiber strain.
ASTM D2412: Standard Test Method for Determination of External Loading Characteristics of Plastic Pipe by Parallel-Plate Loading
ASTM D2412 test method covers the determination of load-deflection characteristics of plastic pipe under parallel-plate loading. It covers thermoplastic resin pipe, reinforced thermosetting resin pipe (RTRP), and reinforced polymer mortar pipe (RPMP). Pipes tested under ASTM D2412 must be smaller than the envelope of the two compression platens by at least a half an inch. Square or circular platens can be used, with most customers choosing a square platen. Care must be taken to account for the mid-section of the pipe which will expand slightly as the pipe is compressed.
The characteristics determined by ASTM D2412 test method are pipe stiffness, stiffness factor, and load at specific deflections.
ASTM D3410 Shear Loading compression Test Method for Compressive Properties of Polymer Matrix Composite Materials with Unsupported Gage Section.
ASTM D3410 measuring in‑plane compressive properties for high‑modulus‑fiber‑reinforced polymer‑matrix composites using pure shear‑loading via wedge grips, with an unsupported gage section on the test coupon. Test method determines the in-plane compressive properties of polymer matrix composite materials reinforced by high-modulus fibers. It is applicable to composites made from unidirectional tape, wet-tow placement, textile (for example, fabric), short fibers, or similar product forms. Some product forms may require deviations from the test method.
Frequently Asked Questions (FAQs) about ISO 899-2 Plastic three-point flexural creep test
Q1. What is ISO 899-2?
ISO 899-2:2024 is the third edition of Plastics — Determination of creep behaviour — Part 2: Flexural creep by three-point loading. It specifies how to measure the time-dependent bending deformation of a freely supported plastic beam under a constant mid-span load, under controlled pre-treatment, temperature and humidity.
Q2. Why is the ISO 899-2 flexural creep test important?
Because plastics are viscoelastic: they keep deforming under a load they easily survive in a short-term test. A bracket, clip, shelf or housing can pass a flexural strength test and still sag, loosen, lose sealing force or rupture months later. ISO 899-2 converts that risk into measurable numbers — deflection, creep strain, creep modulus, compliance and time to rupture — so engineers can design for service life, not just for minute-one strength.
Q3. Why is creep testing important for the material itself?
It reveals how a polymer's stiffness changes with time and environment. Two grades with the same short-term flexural modulus can diverge dramatically after 100 or 1 000 hours. Creep data also expose sensitivity to thermal history, physical ageing, moisture, filler content and fibre orientation — factors that short-term tests hide.
Q4. What does ISO 899-2 actually measure?
Mid-span deflection s_t as a function of time under constant force F. From F, span L, width $b$ and thickness h, the standard calculates flexural stress, flexural-creep strain, flexural-creep modulus E_t, flexural-creep compliance D_t, time to rupture and creep-strength limit.
Q5. Which materials are covered?
Rigid and semi-rigid, non-reinforced, filled and fibre-reinforced plastics, moulded directly or machined from sheets or moulded articles. The method may be unsuitable for some fibre-reinforced materials because of fibre orientation, and it might not apply to rigid cellular plastics — for those, see ISO 1209-1 and ISO 1209-2.
Q6. What industries use ISO 899-2 data?
Automotive and transport, aerospace, building and construction, pipes and geosynthetics, electrical/electronics and appliances, medical devices, renewable energy, and any polymer converter qualifying a long-term loaded part. The standard itself names engineering design, quality control and R&D as the intended uses.
Q7. What is the difference between ISO 899-2 and ISO 178?
ISO 178:2019 is a short-term three-point flexural test at a controlled strain rate; it reports flexural strength and modulus and explicitly says it is not suitable for determining design parameters. ISO 899-2 holds the load constant and observes deformation over time. Same geometry, opposite question: "What happens in a minute?" vs "What happens in a year?"
Q8. What is the difference between ISO 899-1 and ISO 899-2?
Part 1 is tensile creep on dumb-bell specimens; Part 2 is flexural creep on a beam in three-point bending. Bending puts one surface in tension and the other in compression, so a part loaded in bending should be characterised in bending rather than with tensile-creep data.
Q9. What is the ASTM equivalent — ASTM D2990?
ASTM D2990-17(2025) covers tensile, compressive and flexural creep and creep-rupture; flexural creep uses three-point loading per ASTM D790, with optional four-point loading per D6272. ASTM's own note states that D2990 and ISO 899 Parts 1 and 2 address the same subject but differ in technical content, so results cannot be directly compared. ISO 899 does not address compressive creep.
Q10. Do I need a deflectometer, or is crosshead displacement enough?
For engineering-design data, a deflectometer measuring specimen deflection is required. For research or quality-control purposes, the displacement between the loading edge and the supports may be used. Either way, the device must be Class 1 per ISO 9513 and must not influence the specimen mechanically, thermally or chemically.
Q11. Can one machine test several specimens at once?
Yes — creep programmes often run multiple stress levels in parallel, which is why dedicated multi-station dead-weight or constant-force rigs are common. The standard requires that, in creep-to-rupture tests, rupture shocks must not be transmitted to adjacent loading systems.
Q12. How fast is the load applied?
Progressively, so full load is reached between 1 s and 5 s after load application begins. Use the same loading rate for every test in one material series, and count the total load — including any preload — as the test load.
Q13. What measurement schedule does the standard recommend?
1, 3, 6, 12 and 30 min; then 1, 2, 5, 10, 20, 50, 100, 200, 500, 1 000 h, etc. Continuous recording may replace discrete readings, and readings should be taken more frequently if discontinuities appear in the creep curve. Elapsed time must be within ±0.1 % or ±2 s, whichever is less severe.
Q14. How long does an ISO 899-2 test take?
The standard sets no fixed duration; the programme defines it. 1 000 h (about six weeks) is a common design-data horizon, and isochronous curves are normally drawn at 1 h, 10 h, 100 h, 1 000 h and 10 000 h.
Q15. How do I select the right stress level for an ISO 899-2 test?
Stress levels are selected based on the material’s intended application and expected service loads. A mandatory rule from ISO 899-2 is that maximum deflection at any time during the test must not exceed 0.1 times the support span. For engineering design purposes, testing at a minimum of three different stress levels is required to generate isochronous stress-strain curves and creep-to-rupture data.
Q16. Why choose ISO 899-2 Flexural Creep Testing Machines from UnitedTest?
UnitedTest manufactures flexural creep testing machines for ISO 899-2:2024 three-point loading of rigid and semi-rigid plastics. Our creep rigs apply a smooth, reproducible ±1 % constant load to an 80 × 10 × 4 mm specimen, hold a (16 ± 1)h support span, and record mid-span deflection with a Class 1 deflectometer for 1 000 hours or longer. Designed for engineering design, quality control and R&D, UnitedTest systems generate creep curves, creep modulus/time curves, isochronous stress–strain curves and creep-to-rupture data under controlled temperature and humidity.
UnitedTest is a professional manufacturer of high-precision ISO 899-2 flexural creep testing systems, purpose-built for three-point bending creep testing of rigid and semi-rigid plastics in full compliance with ISO 899-2:2024 and EN ISO 899-2:2024 standards. Our plastic creep test equipment delivers accurate, long-term stable measurement of flexural creep modulus, creep compliance, creep strain and creep-to-rupture performance for thermoplastics, mineral-filled compounds, glass/carbon fibre-reinforced polymers and machined or moulded specimens.
Engineered for continuous, maintenance-free operation over extended test durations, UnitedTest three-point bending creep testers feature adjustable support spans, ±1% precision load control, Class 1 deflection measurement per ISO 9513, and optional temperature-controlled environmental chambers for elevated or low-temperature testing. We serve plastics R&D laboratories, quality control departments, automotive component suppliers, aerospace material manufacturers and construction material producers worldwide, providing complete ISO 899-2 test solutions including system integration, calibration, training and ongoing technical support.
Require More Customized Solutions?