Information on the most widely used ASTM standards within the materials testing industry
ASTM D6147 Compression Stress Relaxation Tester | UnitedTest
UnitedTest manufactures ASTM D6147 compression force decay stress relaxation testing machine for vulcanized rubber and TPE, supporting air and liquid environment testing under controlled time and temperature for sealing and elastomer material qualification.
ASTM D6147 specifies two reliable laboratory methods for determining the decrease in counterforce exerted by a test specimen of vulcanized rubber or thermoplastic elastomer (TPE) that has been compressed to a constant deformation under specified conditions of time and temperature. This standard was developed on the basis of testing both in air and in liquids, making it ideal for evaluating sealing rings, gaskets, hoses and other elastic components that need to maintain stable sealing force under long-term compression. It helps material engineers and quality teams predict long-term sealing performance, compare different elastomer formulations, verify batch consistency and support product approval for automotive, plumbing, aerospace and industrial sealing applications. UnitedTest’s ASTM D6147 stress relaxation tester delivers precise force monitoring, stable temperature control and flexible test chamber options to meet your rubber and TPE compression relaxation test requirements.
Test Principle:
When a constant compressive strain is applied to rubber or thermoplastic elastomers, the force required to maintain that fixed deformation decreases over time. This time-dependent phenomenon is formally defined as force decay (stress relaxation). Its mechanical counterpart — deformation increase under constant stress — is known as creep.
Force decay originates from two co-occurring mechanisms:
Physical relaxation: Dominates at ambient/low temperatures or short test durations, driven by viscoelastic rearrangement of polymer molecular chains.
Chemical relaxation: Dominates at elevated temperatures or extended test durations, caused by oxidative degradation, bond scission, or crosslink network changes in the material.
The standard explicitly warns against extrapolating time-decay curves to predict performance far beyond the test window, or using high-temperature tests as accelerated predictors for low-temperature service, due to the shift in dominant decay mechanisms. Initial stress level and prior mechanical history of the specimen also influence results, particularly for filled rubber compounds.
Specific Test Methods
The standard specifies two distinct test methods (Method A and Method B) that produce non-comparable numerical results; method selection is determined by test purpose. A supplementary liquid immersion protocol is also defined.
Method A (In-Situ Temperature Measurement)
All compression operations and force measurements are performed continuously at the target test temperature.
Designed for fundamental material research and applications where high-temperature sealing performance is a critical requirement.
Specimens are never removed from the test temperature environment during measurement.
Method B (Ambient Temperature Measurement After Thermal Aging)
Initial compression and baseline force measurement are carried out at standard laboratory temperature (23 ± 2 °C).
The compressed specimen assembly is placed in an oven at the specified elevated temperature for aging.
For each scheduled time-point measurement, the fixture is removed from the oven, conditioned at standard laboratory temperature for 2 hours (this 2-hour equilibration period is counted toward total test duration), then force is measured at ambient temperature before the specimen is returned to the oven.
Key Parameters and Stipulations
| Compression | 25 ± 1 %; if unattainable, 15 ± 1 % |
| Time to apply compression | ≤ 30 s |
| Compression during test | Fixed and maintained for the entire test period (except the tiny measuring displacement of 6.4) |
| Preheat (Method A) | Specimen and jig preheated to test temperature; ~30 min preheat recommended (per D1349) |
| Initial counterforce F₀ | Measured 30 min after compression, at ±1 % accuracy |
| Test temperature | Chosen from D1349; oven tolerance per D573/E145 |
| Typical test duration | 168 h found suitable for many elastomers; duration otherwise agreed between customer and supplier; longer programmes use a logarithmic time scale |
| Method B equilibration | 2 h at 23 ± 2 °C before each reading, included in test duration |
| Replicate readings | 3 counterforce measurements per specimen per time, median used |
| Immersion fixture ports | Inlet/vent ≥ 3.2 ± 0.3 mm diameter |
| Typical measurement schedule (industrial practice) | e.g. 24, 72, 96, 168, 336, 504, 1008 h, often plotted against log time |
Test Specimen Information:
Three validated specimen types are defined; the washer type is the preferred configuration:
Small cylindrical disc: 13.0 ± 0.5 mm diameter, 6.3 ± 0.3 mm thickness
Large cylindrical disc: 29.0 ± 0.5 mm diameter, 12.5 ± 0.5 mm thickness
Washer-type specimen (preferred): 12.5 ± 0.5 mm inner diameter, 19.0 ± 0.5 mm outer diameter, 2.0 ± 0.2 mm thickness. Thickness variation within a test set must not exceed 0.025 mm.
ASTM D6147 Rubber Compression Stress Relaxation Test required Testing Equipment:
| Compression Device | A jig with two parallel flat plates that compresses and holds specimens at fixed deformation. Construction material must resist degradation from the test environment (e.g., acidic oils). It must apply target compression within 30 seconds, maintain deformation throughout testing, and withstand oven temperatures. Two validated designs (including the Wykeham Farrance Stress Relaxation Fixture) are referenced.
|
| Counterforce Measuring Device | High-accuracy force measurement system:
|
| Oven | Forced-ventilation type with precision temperature control, conforming to ASTM Specification E145. |
| Temperature Reading Device | Thermocouple mounted at the oven center cavity for temperature verification. |
Key Test Procedures of ASTM D6147 Rubber Compression Stress Relaxation Test:
Method A Procedure
Preheat the compression fixture to the target test temperature.
Precondition the specimen at test temperature for a recommended 30 minutes, in accordance with Practice D1349.
Compress the preheated specimen to the specified strain within 30 seconds, then lock the deformation.
After 30 ± 2 minutes of compression, measure the initial counterforce (F0) at test temperature with ±1% accuracy.
Repeat force measurements at predefined time intervals, with all measurements conducted at the test temperature.
For each time point, take 3 readings per specimen and use the median value for calculation.
Method B Procedure
Compress the specimen to the specified strain at 23 ± 2 °C within 30 seconds, then lock the deformation.
After 30 ± 2 minutes, measure the initial counterforce (F0) at standard laboratory temperature.
Place the compressed fixture assembly into the oven at the target elevated temperature.
At each scheduled time point:
Remove the fixture from the oven
Condition at standard laboratory temperature for 2 hours (included in total test duration)
Measure counterforce
Return the fixture to the oven to resume aging
Take 3 readings per specimen per time point and use the median value.
Industries application:
This test is widely used in sectors where rubber/elastomer components operate under sustained compressive load:
Sealing and gasket manufacturing: O-rings, static gaskets, and sealing elements for automotive, aerospace, oil and gas, plumbing, and industrial piping systems
Rubber material R&D: Formulation optimization, filler effect evaluation, and aging resistance development
Quality control: Batch consistency verification for compounded rubber and thermoplastic elastomer production
Fluid system engineering: Evaluation of seal performance when exposed to oils, fuels, hydraulic fluids, or chemical media
Electronics and appliance engineering: Sealing components for electrical enclosures, connectors, and household appliances

Related Test Standard
| ASTM D695 | Standard Test Method for Compressive Properties of Rigid Plastics |
| BS 903 Part A34 | British ring‑specimen method, including measurement under immersed conditions |
| ASTM D3410 | Shear‑loading compression test for polymer‑matrix composites with unsupported gauge section, suited for high‑strength continuous‑fiber composite laminates (not pure end‑loading as D695). |
| ASTM D575 | Standard Test Methods for Rubber Properties in Compression. |
| ISO 7616 | Cellular plastics, rigid-Determination of compressive creep under specified load and temperature conditions |
| ISO 6056 | Compression stress relaxation specifically for O‑rings / rings. |
| ASTM D6147 | Rubber Compression Stress Relaxation Test |
| ISO 3384-1/ ISO 3384-2 | The corresponding international standard series for vulcanized rubber compression stress relaxation; covering both constant-temperature measurement and intermittent ambient-temperature measurement procedures. |
| ISO 604 | Plastics -- Determination of compressive properties |
| ISO 7743 | Rubber, vulcanized or thermoplastic; determination of compression stress-strain properties |
| ASTM D573 | Test Method for Rubber – Deterioration in an Air Oven (reference for oven conditioning protocols) |
| JIS K 6254 | Japanese standard for compression and tensile stress–strain properties. It is MOD relative to ISO 7743 |
| ISO 815-1 | Compression set at ambient or elevated temperatures . It measures permanent deformation after prolonged compression, not short-term stress–strain behaviour. |
| ASTM D4483 | Practice for Evaluating Precision for Test Method Standards in the Rubber and Carbon Black Manufacturing Industries (provides precision analysis framework) |
| ASTM E145 | Specification for Gravity-Convection and Forced-Ventilation Ovens (defines oven performance requirements) |
Keywords: ASTM D6147 tester, compression stress relaxation tester, rubber force decay tester, vulcanized rubber stress relaxation test, TPE compression relaxation testing machine, gasket stress relaxation test, elastomer sealing performance test, rubber compression set relaxation tester, stress relaxation equipment for rubber, ASTM D6147 test machine, rubber material testing instrument, sealing component durability test, liquid immersion stress relaxation tester, automotive rubber seal test, industrial elastomer quality control tester
Related products and device
Related Standard
ISO 3384-1 Rubber, vulcanized or thermoplastic — Determination of stress relaxation in compression — Part 1: Testing at constant temperature
ISO 3384-1 specifies standardized laboratory procedures to measure the reduction in counterforce exerted by vulcanized or thermoplastic rubber specimens held under constant compressive deformation at a defined test temperature, valid for both gaseous and liquid test environments.
ASTM D695: Standard Test Method for Compressive Properties of Rigid Plastics
ASTM D695 test covers the determination of the mechanical properties of unreinforced and reinforced rigid plastics, including high-modulus composites, when loaded in compression at relatively low uniform rates of straining or loading. Test specimens of standard shape are employed. This procedure is applicable for a composite modulus up to and including 41,370 MPa (6,000,000 psi). It is technically equivalent to ISO 604 Plastics‑Determination of Compressive Properties. This test applies end‑loading compression on standard‑geometry specimens under controlled environmental and displacement‑rate conditions, delivering compressive strength, yield strength, offset yield strength, compressive elastic modulus, and compressive deformation data.
ASTM D2412: Standard Test Method for Determination of External Loading Characteristics of Plastic Pipe by Parallel-Plate Loading
ASTM D2412 test method covers the determination of load-deflection characteristics of plastic pipe under parallel-plate loading. It covers thermoplastic resin pipe, reinforced thermosetting resin pipe (RTRP), and reinforced polymer mortar pipe (RPMP). Pipes tested under ASTM D2412 must be smaller than the envelope of the two compression platens by at least a half an inch. Square or circular platens can be used, with most customers choosing a square platen. Care must be taken to account for the mid-section of the pipe which will expand slightly as the pipe is compressed.
The characteristics determined by ASTM D2412 test method are pipe stiffness, stiffness factor, and load at specific deflections.
ASTM D3410 Shear Loading compression Test Method for Compressive Properties of Polymer Matrix Composite Materials with Unsupported Gage Section.
ASTM D3410 measuring in‑plane compressive properties for high‑modulus‑fiber‑reinforced polymer‑matrix composites using pure shear‑loading via wedge grips, with an unsupported gage section on the test coupon. Test method determines the in-plane compressive properties of polymer matrix composite materials reinforced by high-modulus fibers. It is applicable to composites made from unidirectional tape, wet-tow placement, textile (for example, fabric), short fibers, or similar product forms. Some product forms may require deviations from the test method.
ISO 14126 Compression test Fibre-reinforced plastic composites — Determination of compressive properties in the in-plane direction
ISO 14126 specifies how to determine in‑plane compressive properties (i.e. load applied parallel to the plane of lamination, in directions "1" and "2") of fibre‑reinforced plastic composites with thermosetting or thermoplastic matrices. Specimens are machined from a flat test plate or from finished/semi‑finished products.
ISO 604 specifies a method for determining the compressive properties of plastics under defined conditions. It is used to investigate the compressive behavior of test specimens and to determine key mechanical properties such as compressive strength, compressive modulus, and other aspects of the compressive stress/strain relationship. Specimen length is adjusted to avoid buckling that would distort results.
ASTM D575 Standard Test Methods for Rubber Properties in Compression
ASTM D575 defines two laboratory test procedures to characterize the compression‑deflection behavior of solid rubber compounds. It does not apply to hard rubber or sponge rubber materials. It contains two inverse procedures: Method A fixes the deflection and measures the force; Method B fixes the force and measures the deflection.
ISO 7743 Rubber, vulcanized or thermoplastic — Determination of compression stress-strain properties
ISO 7743 defines standardized methods for measuring the compression stress-strain properties of vulcanized or thermoplastic rubber, applicable to standard laboratory test pieces, finished products, or product segments.
Frequently Asked Questions (FAQs) about ASTM D6147 Rubber Compression Stress Relaxation Test
Q1. What is ASTM D6147?
A: ASTM D6147 is the ASTM International test method that measures how much the counterforce (reaction force) of a compressed vulcanized rubber or thermoplastic elastomer (TPE) specimen decreases over time while the deformation is held constant. It specifies two procedures (Method A and Method B), and covers testing in both air and liquids.
Q2. What do "force decay", "stress relaxation" and "creep" mean?
A: Under a constant strain, the force needed to hold that strain falls with time — that is force decay, also called compression stress relaxation. The opposite case, where a constant stress causes deformation to grow with time, is creep. D6147 measures the first phenomenon.
Q3. Why is the ASTM D6147 test important for rubber materials?
A: Because it measures the property that actually keeps a joint sealed: residual contact pressure. A gasket or O‑ring can look dimensionally unchanged yet quietly lose the force pressing against the mating surface until the joint leaks. D6147 turns that invisible loss into a quantifiable force‑retention curve, so engineers can compare compounds, qualify suppliers, set design margins, estimate service life and schedule seal replacement before a field failure occurs. It also separates early reversible physical relaxation from irreversible chemical ageing (oxidation, chain scission, crosslink breakdown), which is essential for formulation development and failure analysis.
Q4. Why is stress relaxation more meaningful than compression set for seals?
A: Compression set (ASTM D395 / ISO 815‑1) measures permanent thickness loss after the load is removed. Stress relaxation (ASTM D6147) measures the sealing force while the part stays compressed in service. A material can show excellent recovery after unloading but poor force retention under load — the two properties are not equivalent. For long‑term static sealing, force retention is the more direct predictor of leak‑free performance. Best practice is to run both.
Q5. Which materials and products is D6147 used for?
A: Vulcanized rubber and thermoplastic elastomers used for O‑rings, gaskets, static and dynamic seals, flange and valve seals, weatherstrips, hydraulic/pneumatic seals, engine‑bay and fuel‑system seals, EV battery enclosure gaskets, cable and switchgear seals, and medical or aerospace sealing components.
Q6. What is the difference between Method A and Method B?
A: In Method A, the specimen is compressed, aged and all force measurements are made at the test temperature — ideal for continuous hot service and fundamental studies. In Method B, compression and the initial reading happen at 23 ± 2 °C, the specimen is aged in an oven at the test temperature, then cooled to 23 ± 2 °C for 2 h before every reading — better for temperature‑cycling service and for labs without in‑oven force measurement.
Q7. What specimens are used, and which is preferred?
A: Three standard geometries: a Ø13.0 × 6.3 mm disc, a Ø29.0 × 12.5 mm disc, and a washer (ID 12.5 mm / OD 19.0 mm / 2.0 mm thick). Other sizes may be used if the end use dictates. The washer type is preferred by the standard and is the best choice for immersion work. Because of the shape factor, results from different shapes/sizes are not equivalent.
Q8. How do I choose between Method A and Method B?
A: Choose Method A when the seal works continuously at elevated temperature or when you need the true in‑service force profile. Choose Method B when the application involves cycling between ambient and elevated temperature, or when high‑temperature in‑situ force measurement is impractical (common in quality control).
Q9. What compression level is applied?
A: 25 ± 1 % of the original thickness. If 25 % cannot be achieved, 15 ± 1 % is permitted. The compression must be applied within 30 s and then locked and maintained for the entire test, except for the tiny extra displacement used to take a reading.
Q10. When is the initial counterforce F₀ measured?
A: 30 minutes after compression is applied, measured with ±1 % accuracy. This F₀ is the denominator for all subsequent force‑decay calculations.
Q11. What are the most common sources of poor repeatability?
A: Inconsistent temperature control or heat loss through jig metalwork, compression not locked at exactly the same value, variation in initial stress or mechanical history (especially with filled rubbers), dirty plates or mould release on the specimen, inconsistent 2 h thermal equilibration in Method B, and uncalibrated force measurement. Section 13 reports a 1994 interlaboratory programme (7 labs, one compound, air at 70 °C) with repeatability/reproducibility tables at 24, 96 and 168 h; bias cannot be determined because the property is defined only by the method.
Q12. Why choose UnitedTest ASTM D6147 Compression Stress Relaxation Test System?
UnitedTest manufactures high-precision ASTM D6147 compression force decay testing machines for vulcanized rubber and thermoplastic elastomers. Method A & Method B compliant, with liquid immersion capability. Reliable stress relaxation test equipment for seal and gasket quality control.
UnitedTest is a leading manufacturer of advanced material testing equipment specializing in rubber and elastomer characterization. Our ASTM D6147 compression stress relaxation tester delivers precise, repeatable force decay measurements for vulcanized rubber and thermoplastic elastomer specimens under controlled compression, time, and temperature conditions.
Engineered to fully comply with ASTM D6147-97 (2020) standard requirements, the UnitedTest system supports both Method A (in-situ temperature measurement) and Method B (ambient temperature measurement after thermal aging) test protocols. The equipment accommodates all three standard specimen geometries — cylindrical discs and washer-type specimens — and features an optional liquid immersion chamber for evaluating seal performance in oils, hydraulic fluids, and chemical media.
High-precision force measurement with accuracy better than 0.5% of full scale, meeting ASTM D6147 counterforce measurement requirements
Temperature-controlled oven conforming to ASTM E145 with forced ventilation and uniform temperature distribution
Programmable test durations with automatic data logging at user-defined time intervals
Digital displacement control ensuring accurate 25% or 15% compression applied within 30 seconds
Integrated thickness measurement per ASTM D3767 for specimen preparation verification
UnitedTest Pro-Soft software for real-time force decay curve display, automatic calculation of R(t) and FR(t), and customizable test reports
UnitedTest ASTM D6147 testing machines serve quality control laboratories, R&D centers, and rubber product manufacturers worldwide in the automotive sealing, aerospace gasket, oil and gas, plumbing, and industrial elastomer sectors. Whether you are conducting material formulation development, batch quality verification, or long-term sealing performance validation, our stress relaxation test system provides the accuracy and reliability you need.
Require More Customized Solutions?