Home >> Application >> By Standard >> Others >> EN 10233 Tube Flattening Test Method, Specimen, Equipment and Test Machines

EN 10233 Tube Flattening Test Method, Specimen, Equipment and Test Machines

Share:

EN 10233 Metallic Tube Flattening Test Machine | UnitedTest

UnitedTest manufactures EN 10233 compliant flattening testers for circular metallic tubes up to D 600 mm. Evaluate plastic deformation and detect laminations, weld flaws and cracks in metal tubing for industrial quality control.


EN 10233 Metallic materials specifies the tube flattening test to assess the plastic deformation performance of circular cross-section metallic tubes. This test also identifies internal defects including laminations, weld flaws, cracks and discontinuities. It applies to tubes with outer diameter D ≤ 600 mm and wall thickness T ≤ 15 % of D. UnitedTest provides reliable EN 10233 flattening test rigs for steel pipe manufacturers, tubing fabricators and independent material testing laboratories.


Test Principle: 

A test piece — either cut from a tube or the end of a full-length tube — is compressed perpendicular to the tube's longitudinal axis, between two platens, until the distance H between the platens, measured under load, reaches the value specified in the product standard.

For close (full) flattening, the inner surfaces must be in contact over at least half of the internal width b of the flattened test piece.


Test Specimen Information:

  • Length: 10 mm ≤ specimen length L ≤ 100 mm. Specimen edges may be filed rounded or chamfered; un‑processed edges are acceptable if test criteria are satisfied.

  • When testing on the end of full‑length tube: cut the tube end perpendicular to its axis, with cutting depth at least 80 % of tube outer diameter D.

  • Applicable tube dimension range: outer diameter D ≤ 600 mm; wall thickness T ≤ 15 % of outer diameter D. Product standards may define narrower dimensional limits for specific tubes.


EN 10233 Metal Tube Flattening Test required Testing Equipment: 

Test Machine

A machine capable of flattening the test piece to the prescribed distance H between two plane, parallel, rigid platens. 

In practice this is a compression / universal testing machine (or a dedicated press) of adequate capacity and stiffness.

Compression platens

Platen width must exceed the width of the flattened test piece — at least 1.6 D; platen length must extend over the whole length of the test piece. 

EN 10233 Tube Flattening Test Method, Specimen, Equipment and Test Machines


Key Parameters and Stipulations

SymbolDescriptionUnit
DOutside diameter of the tubemm
TWall thickness of the tubemm
bInside width of the flattened test piecemm
LLength of the test piecemm
HDistance between platens, measured under loadmm

H is THE controlling parameter of the test; the product standard normally defines H either as a fixed value, as a fraction of D, or by a formula such as H = (1+e)T / (e + T/D), where e is a deformation-per-unit-length constant dependent on steel grade (this formula form is used in ASTM A530/A530M practice).


Key Test Procedures:

  1. Place specimen between the two parallel platens.

  2. For welded tubes: position the weld location as required by the corresponding product standard.

  3. Drive platens to compress the specimen perpendicular to tube longitudinal axis.

  4. In case of dispute: platen moving rate shall not exceed 25 mm/min.

  5. Result assessment: follow product‑standard requirements. Without specified rules: specimen passes if no visible cracks without magnification. Minor edge cracking alone is not a rejection reason.

  6. When required, issue a test report including: standard reference, specimen identification, specimen dimensions, flattening degree, weld position, and test result.


Industry Application Fields:

The flattening test is a low-cost, high-information technological (technological/ductility) test applied to essentially every sector that uses circular metallic tube:

  • Pressure equipment & boilers: seamless and welded steel tube for boilers, superheaters, heat exchangers, pressure piping (e.g. EN 10216 / EN 10217 families, GB/T 5310, GB/T 9948). Confirms the tube can survive forming (bending, expanding into tube sheets) without cracking.

  • Oil, gas & petrochemical: line pipe, casing and refinery/petrochemical process tube — the test screens for longitudinal seams, laminations and lack of fusion in welded pipe.

  • Structural & mechanical tubing: hollow sections, hydraulic cylinders, automotive and machinery tube; also referenced for structural hollow sections (ASTM A500/A500M) and general pipe requirements (ASTM A530/A530M, A450/A450M, A999/A999M, A1016/A1016M).

  • Aerospace and non-ferrous tube: BS EN 10233 is referenced by aerospace test-method documents (e.g. BS 5A 4-4, plastic deformation tests on tubes) and by copper-alloy tube specifications such as BS 3B 27 / BS 2B 27. Because the standard is written for "metallic materials" generally, it applies equally to carbon steel, alloy steel, stainless steel, copper, aluminium and titanium alloys.

  • Tube-making process control: a rapid mill-floor check on weld quality for ERW/HFI welded tube, and on annealing/ductility of cold-drawn tube (e.g. EN 10305 precision tube families). 


Related standard: 

EN 10232Metallic Materials - Tube (in Full Section) - Bend Test
IS 2328 (India standard) — corresponds to ISO 8492
ASTM B968flattening of copper and copper-alloy pipe and tube.
ISO 7438General bend test for flat metal strip/sheet specimens.
TCVN 5891Metallic materials. Tube (in full section).Bend test
ISO 8491Tube (in full section) bend test, bend rather than flatten
ISO 8492Metallic materials. Tube. Flattening test
ISO 8493Metallic materials - Tube - Drift-expanding test

GOST 8695

Metal pipes. Flattening testing method
EN 10233Metallic materials. Tube. Flattening test
GB/T 246Metallic materials—Tube—Flattening test
DIN 50136

German Flattening test


Why This Test Matters for a Material

  1. Evaluate ductility & plastic deformation capacity: It verifies whether tubular material can sustain plastic compression deformation without cracking, reflecting material ductility for forming service conditions.

  2. Detect manufacturing defects: The flattening stress exposes hidden defects such as weld cracks, laps, seams, inclusions and brittleness originating from tube production (welding, rolling, heat‑treatment).

  3. Verify product quality compliance: It serves as a mandatory acceptance test for many tubular product specifications, to confirm tubes meet safety and mechanical‑performance requirements before delivery.

  4. Simulate practical deformation risks: It reflects material behaviour under compressive bending‑flattening load that tubes may encounter during installation, transportation or service, preventing early in‑service fracture failure


Keywords: EN 10233 tester, metallic tube flattening test machine, metal pipe flattening tester, steel tube flattening test rig, welded pipe defect inspection tester, circular metal tube plastic deformation test equipment, seamless tube flattening quality test fixture, pipe weld crack detection tester, large diameter metal tube flattening machine, tubular product mechanical property tester, alloy tubing flattening verification system, industrial metal tube quality inspection equipment

Related products and device

EN 10233 Metal Tube Flattening Test Universal Testing Machine

WDW Series Computer Control Electronic Universal Testing Machine made by UNITEDTEST range from 100N to 600KN load capacity with various models like single columns, table type, door frame type etc., is used to perform tension, compression, flexure/bending, shearing, peeling etc., test for metal and nonmetal specimens.

EN 10233 pipe weld crack detection tester, large diameter metal tube flattening machine

Compression test fixture is used to investigate the compressive behaviour of the test specimens and for determining the compressive strength, compressive modulus and other aspects of the compressive stress/strain relationship under the conditions defined.

Related Standard

ISO 8492 Metal Tube Flattening Test –

ISO 8492 Metallic materials — Tube — Flattening test

ISO 8492 is a method for determining the ability of metallic tubes of circular cross-section to undergo plastic deformation by flattening; it may also be used to reveal defects in the tubes. ISO 8492 defines how to flatten; how far to flatten (distance H), where the weld goes, and what counts as failure are delegated to the relevant product standard or purchase order.

ISO 8491 Metal Tube Bend Test –

ISO 8491 define a unified bend test method for evaluating the plastic bending ductility of circular full-section metallic tubes, exclusively for tubes with outer diameter D ≤ 65 mm (product standards may narrow this diameter range further). 

Main Industry fields: boilers & pressure vessels, oil & gas pipelines, automotive (exhaust/chassis tubing), heat exchangers, structural steel tubing, power generation (including nuclear).

ISO 8493 Metal Tube Drift Expanding Test –

ISO 8493 Metallic materials - Tube - Drift-expanding test

ISO 8493 specifies a method for determining the ability of metallic tubes of circular cross-section to undergo plastic deformation in drift expansion.

Applicability limits (default, unless the relevant product standard narrows them further):

  • Outside diameter D ≤ 150 mm (≤ 100 mm for light metals such as aluminium alloys)

  • Wall thickness a ≤ 10 mm


EN 10232 Metallic Tube Bend Test in Full Section –

EN 10232 is the European version of ISO 8491,defines a unified cold bend test for intact circular full-section metallic tubes, designed to quantify plastic bending ductility for tubes with outer diameter D ≤ 65 mm. 

ASTM A500 Cold-Formed Steel Tube & Section Mechanical Testing –

ASTM A500 covers carbon steel tubing in round, square, rectangular, or special shapes, primarily used for welded, riveted, or bolted construction in bridges, buildings, and general structural applications. It specifies four mandatory test categories, tension test, flattening test, Chemical Composition Analysis and Dimensional & Visual Inspection.  For us, will focus on the mechanical test. 

ASTM D2105 Longitudinal Tensile Test for Fiberglass Pipe & Tube –

ASTM D2105 Standard Test Method for Longitudinal Tensile Properties of "Fiberglass" (Glass‑Fiber‑Reinforced Thermosetting‑Resin) Pipe and Tube

ASTM D2105 determine the comparative longitudinal tensile properties of a fiberglass pipe specimen by pulling it in axial tension to failure under defined conditioning, temperature, and machine‑crosshead‑speed conditions.

ASTM F2663 – Bead Unseating of Tubeless Passenger and Light Truck Tires –

ASTM F2663 Standard Test Method for Bead Unseating of Tubeless Passenger and Light Truck Tires

ASTM F2663 quantify the resistance of tubeless tires against bead unseating, which means the tire bead slipping off the rim flange leading to sudden air loss. It covers passenger tires, light‑truck tires, and temporary spare tires. It only defines test methodology, not mandatory performance limit values for tires.

ASTM A370 Test method for mechanical testing of steel –

ASTM A370 Standard Test Methods and Definitions for Mechanical Testing of Steel Products


ASTM A370 test methods cover procedures and definitions for the mechanical testing of steels, stainless steels, and related alloys. The various mechanical tests herein described are used to determine properties required in the product specifications. Variations in testing methods are to be avoided, and standard methods of testing are to be followed to obtain reproducible and comparable results. In those cases in which the testing requirements for certain products are unique or at variance with these general procedures, the product specification testing requirements shall control.


Covering tests like Tension, Bend, Hardness, Brinell, Rockwell, Portable, and Impact, each catering to distinct aspects of mechanical property assessment. Moreover, it accommodates annexes for specific product types, including Bar Products, Tubular Products, Fasteners, Round Wire Products, and more, ensuring a holistic approach to testing.


FAQs for EN 10233 Metallic Materials‑Tube‑Flattening Test

Q1: Why is the EN 10233 tube flattening test important?

A: This destructive mechanical test serves two core purposes. First, it evaluates the plastic deformation ductility of circular metallic tubes, verifying whether tubes can withstand compression‑flattening without cracking. Second, it exposes hidden manufacturing defects such as weld cracks, laps, seams, inclusions and brittleness introduced during rolling, welding or heat‑treatment. It is a mandatory acceptance check for welded & seamless tubes for pipeline, pressure components and structural applications, preventing premature service failure during transport, installation or operation.


Q2: What tube dimensions are covered by EN 10233?

A: It applies to circular tubes with outer diameter D ≤ 600 mm, wall thickness T ≤ 15 % of outer diameter D. Individual product standards may define narrower dimensional limits for specific tube grades and uses.


Q3: What is the valid specimen size for EN 10233 flattening test?

A: Specimen length L must be between 10 mm and 100 mm. Specimen edges may be filed rounded or chamfered; un‑processed sharp edges are permitted if test results meet acceptance criteria. When testing the end of full‑length tube, cutting depth shall be at least 80 % of tube outer diameter D.


Q4: What are platen requirements for EN 10233 test equipment?

A: Two flat, parallel, rigid platens are required. Platen width ≥ 1.6 × tube outer diameter D to fully cover specimen width after flattening; platen length must fully cover the full length of test piece to ensure uniform compression load.


Q5: What industries commonly apply EN 10233 flattening test?

A: Steel tube manufacturing, non‑ferrous metal tube (aluminium, copper), pressure pipeline, mechanical structural tubing, automotive tubing, construction pipe, quality inspection laboratories, third‑party certification labs, incoming‑goods QC departments.


Q6: What is the maximum platen moving speed when disputes occur?

A: In case of disagreement on test results, platen movement rate shall not exceed 25 mm/min. For routine non‑disputed testing, speed is defined by relevant product specifications.


Q7: How to handle welded tubes during flattening test?

A: Weld position shall follow requirements from corresponding product standard. The weld can be placed at 0°, 90° or other angles relative to flattening direction as specified, to verify weld ductility and detect weld‑zone cracking. Weld position must be recorded in final test report.


Q8: How do we judge pass / fail for EN 10233 flattening test?

A: Evaluation rules are defined by product standards. If no product‑specific rules are given: specimen passes if no visible cracks observed by naked eyes (without magnification). Slight small cracking only at specimen edges shall NOT be taken as rejection grounds.


Q9: What is “close flattening” condition in EN 10233?

A: For close‑flattening requirement, the inner surfaces of flattened specimen must maintain contact over at least half of the flattened inner width b. This is a special acceptance criterion for some tube product specifications.


Q10: What mandatory content must be included in EN 10233 test report?

A: (1) Standard reference EN 10233; (2) Specimen identification; (3) Specimen dimensions (D, T, L); (4) Degree of flattening / platen gap H; (5) Weld position for welded tubes; (6) Final test result (pass / fail).


Q11: Which standard is EN 10233 derived from? What is its successor?

A: EN 10233 was adapted from ISO 8492:1986, with editorial revisions, updated symbol system referencing ISO 3545‑1:1989, and partial drawing referenced from DIN 50136. This standard is now superseded by EN ISO 8492 series, which remains the current global tube flattening test standard.


Q12: Can I use universal compression test machine for EN 10233 flattening test?

A: Yes, but you must install qualified parallel rigid platens meeting platen width ≥ 1.6 D requirement. Ordinary compression platens that are too narrow will create edge stress distortion and produce invalid test results.


Q13: Why choose EN 10233 Tube Flattening Testing Machine from UnitedTest Manufacturer?

A:  UnitedTest is professional manufacturer of EN 10233 tube flattening testing machine, compliant with EN 10233, EN ISO 8492 for metallic seamless & welded tube flattening test. Reliable compression platens, controlled test speed, full test report output for metal tube quality control lab. Customizable capacity & platen size for tube outer diameter up to 600 mm.


UnitedTest is a trusted global manufacturer of metallic tube flattening testing machines fully compliant with EN 10233 (BS EN 10233:1994) and updated EN ISO 8492 standards for circular metal tube flattening test.

Our flattening test equipment is designed to perform radial compression flattening tests for seamless tubes and welded tubes, to evaluate plastic deformation capacity and detect hidden defects including weld cracks, laps and material brittleness. Suitable for steel, aluminium, copper and other non‑ferrous metallic tubes with outer diameter up to 600 mm.

Core machine features meeting EN 10233 requirements

  1. Heavy‑duty parallel rigid platens: platen width ≥ 1.6 × tube outer diameter D, fully covering specimen after flattening to eliminate edge stress distortion.

  2. Precise platen movement speed control: adjustable speed down to ≤ 25 mm/min for dispute‑condition testing as required by EN 10233.

  3. Temperature‑compatible operation for lab ambient 10 ~ 35 °C, supports controlled testing at 23±5 °C.

  4. Software automatically records test parameters: tube outer diameter D, wall thickness T, specimen length L, platen‑to‑platen distance H, weld position, flattening degree and test result. Directly generate EN 10233‑compliant test reports for lab certification and product acceptance.

  5. Multiple safety protection: overload protection, displacement limit stop, emergency stop button for lab daily operation.

  6. Customizable options: different load force capacity, platen dimension, hydraulic or servo‑electric loading system to match your tube dimension range.

Typical application scenarios

  • Tube manufacturing factory in‑house quality control

  • Third‑party material testing laboratories & certification institutions

  • R&D lab for new tube material & welded tube process development

  • Incoming inspection for pipeline, pressure component, automotive and construction tubular parts

UnitedTest provides complete one‑stop solution including machine hardware, standard‑compliant test software, installation, training and after‑sales support. Contact us for quotation for your EN 10233 tube flattening test project.

< Previous: EN 10234 Drift Expanding Test for Metallic Tubes

> Next: EN 1842 Compression Moulding Shrinkage Test of plastics compounds

Require More Customized Solutions?

We offer customization to meet your specific needs. Our expert team will collaborate with you to develop the perfect product for you
Customize Now