ISO 1133 Test Mehod of Determination the melt mass-flow rate (MFR, MVR)
Date:2017-02-19 Source:United Test Views:100

ISO 1133 Test Mehod of Determination the melt mass-flow rate (MFR, MVR)


ISO 1133: Plastics -- Determination of the melt mass-flow rate (MFR) and the melt volume-flow rate (MVR) of thermoplastics.

This standard specifies two procedures for the determination of the melt mass-flow rate (MFR) and the melt volume-flow rate (MVR) of thermoplastic materials under specified conditions of temperature and load. One is a mass-measurement method. The other is a displacement-measurement method. Normally, the test conditions for measurement of melt flow rate are specified in the material standard with a reference to ISO 1133. The test conditions normally used for thermoplastics are listed in annexes. 


There two accurate ISO tests, primarily used for quality control and performed under specified temperature conditions, can be described as: 

Procedure A – a mass-measurement method  Or MFR. 

Procedure B – a displacement-measurement method. Or MVR. 

Melt volume flow rate testing is particularly useful when inspecting materials of different filler content and when comparing filled, with unfilled, thermoplastics. Mass flow rate testing can be determined from melt volume flow rate testing measurements, or vice versa, provided the melt density at the test temperature is known. 


The thermoplastics materials industry uses the Melt Flow Index (MFI) as a basic tool for quality control and acceptance of incoming products. The measure of the flow properties is contained on the identity card, and is used as a check to verify if the plastic's grade is within the required fluidity range. This is commonly used for polyolefins (polyethylene HDPE, LDPE, LLDPE, and polypropylene PP).

\    \

Common Melt Flow Rate Conditions by Material:


MaterialCondition
PS200/5.00
PE190/2.16
190/0.325
190/21.60
190/5.00
PP230/2.16
ABS220/10.00
PS-I200/5.00
E/VAC150/2.16
190/2.16
125/0.325
SAN220/10.00
ASA, ACS, AES220/10.00
PC300/1.20
PMMA230/3.80
PB190/2.16
PB190/10.00
POM190/2.16
MABS220/10.00


Related products
Contact

Email:
export@unitedtest.com
unitedtest@hotmail.com
Tel:
+86-10-57055071
+86-13911165373

MS Teams: 
unitedtest@hotmail.com

WhatsApp:
+86 13911165373

WeChat:
UnitedTest-V1 

X