UnitedTest manufactures ISO 11343 wedge impact testing machines for high-strength structural adhesive joints. This dynamic wedge impact test evaluates cleavage resistance, impact force and fracture energy under crash-rate loading for automotive composite and metal bonded assemblies.
ISO 11343 Adhesives — Determination of dynamic resistance to cleavage of high-strength adhesive bonds under impact wedge conditions — Wedge impact method. ISO 11343 defines a high‑rate dynamic wedge‑impact test to characterize impact cleavage performance of high‑strength structural adhesive joints under impact loading. It measures how much force and energy is needed to split a bonded joint at crash-like speed by driving a hardened-steel wedge between the two adherends. Widely used for structural adhesive R&D, batch quality control and crash performance assessment for automotive, aerospace and composite bonding applications.
Test Principle:
A hardened-steel wedge, moving at high speed, is driven into the bondline between two bonded adherends. The wedge converts the impact into an opening (Mode I / cleavage–peel) stress that initiates a crack at the bondline and propagates it until the two adherends separate. The instrumented machine records force vs. time (or vs. displacement) throughout the few-millisecond event, from which the cleavage force and fracture/cleavage energy are derived.
The wedge is held in a support frame with vertical freedom, so it self-aligns with the bondline during impact. Its included angle, leading-edge radius and maximum depth control how the joint opens ahead of the wedge tip.

Specific Test Methods
| Method A (Stationary Frame Method) | One end of the specimen is rigidly clamped to the fixed frame. The other end is attached to a rigid, fixed‑mass crosshead (yoke). A pendulum strikes the crosshead, accelerating it suddenly and pulling the specimen in tension until fracture. |
Method B (Specimen‑in‑Head Method) aligned with ASTM D1822 | The specimen is mounted inside the pendulum head. A crosshead attached to the free end stops abruptly at impact. The pendulum continues moving, stretching the specimen to failure in tension. |
Test equipment and jig used:
| Instrumented impact‑testing machine | Tensile‑impact pendulum machine (compliant with ISO 13802); Three acceptable machine types: pendulum impact machine, falling‑weight machine, servohydraulic impact tester. - Minimum impact energy ≥ 50 J; minimum impact speed ≥ 2 m/s. - Equipped with specimen clamping grips with 8 mm locating holes for hardened‑steel clamping bolts. - Force‑sensing transducer (piezoelectric, strain gauge etc.) with very fast response time, plus computer/microprocessor for signal recording and post‑processing. - Servohydraulic machines output both force‑time and force‑displacement data; pendulum/falling‑weight devices mainly output force‑time curves. |
| Hardened‑steel test wedge | Two versions: symmetric wedge and asymmetric wedge. Wedge tip radius R1 ± 0.1 mm. Wedge surface must be clean and undamaged; deformed wedges shall be replaced. |
| Wedge support frame | two parallel steel bars plus impact crosshead; total assembly mass 820 g ± 5 g. |
| Thickness measuring device | accuracy ± 0.01 mm for measuring adherend and adhesive layer thickness. |
Test Procedure of ISO 11343 Impact Wedge Peel Test for Adhesives:
Mount the specimen into the wedge fixture; hand‑tighten the specimen‑retaining bolt, then turn an extra quarter‑turn with tool. Position wedge as close as possible to bondline. Stabilize specimen at target test temperature before impact.
Perform impact test. The system automatically records force‑time or force‑displacement signals.
Discard invalid tests:
Bolt mounting hole elongated or adherend fractures near bolt hole (clamping deficiency).
Highly irregular force curves without identifiable cracking and stable‑crack segments.
Post‑processing: identify cracking‑force point and final separation point from recorded curves. Low‑pass signal filtering is permitted for resonant oscillation noise, but filter type and parameters must be documented in report.
Compute results: average cleavage force, dynamic resistance to cleavage (kN/m = average cleavage force / specimen width), dynamic cleavage energy by integrating force‑displacement data over the valid stable‑crack zone (exclude first 25 % and last 10 % of curve).
Specimen information:
Adherend materials: sheet metal or fibre‑reinforced plastic. Adherend thickness range: 0.6 mm‑1.7 mm.
Specimen width: preferred width 20 mm; alternative widths allowed if reported in test report.
Wedge selection rule:
Symmetric wedge: for identical adherends (not always suitable for high‑strength steel or FRP).
Asymmetric wedge: for dissimilar adherends (different thickness, modulus or yield strength). Place higher‑modulus / higher‑yield / thicker adherend on the wedge flat bottom side.
Surface preparation: follow adhesive manufacturer instructions or EN 13887 for metal/plastic surface pretreatment.
Adhesive bond: maximum allowed bond‑line thickness 2 mm; dimension variation within specimen set ≤ 5 %. Remove excess adhesive at wedge entry location to avoid distorting cracking‑force results.
Specimen quantity: test minimum 5 valid replicates.
Specimen geometry: adherend ends are bent for machine clamping; bending configuration must be documented, as bend radius influences test outcomes.
Key test parameter:
| Nominal impact velocity | Typical 2 m/s; actual velocity shall be reported |
| Minimum impact energy | ≥ 50 J |
| Wedge tip radius | R1 ± 0.1 mm |
| Adherend thickness | 0.6‑1.7 mm |
| Max adhesive thickness | 2 mm |
| Specimen width | Preferred 20 mm |
| Number of specimens | ≥ 5 |
| Data evaluation range | Average force calculated between first 25 % and last 10 % of stable‑crack curve region |
Related Test Standard:
| ISO 11343 | Adhesives — Determination of dynamic resistance to cleavage of high-strength adhesive bonds under impact wedge conditions — Wedge impact method |
| GB/T 36877 | (China) — "Determination of impact peel strength of structural adhesives — Wedge method", a modified adoption of ISO 11343 |
| ISO 25217 | mode I adhesive fracture energy G_IC by DCB/TDCB (quasi-static fracture mechanics counterpart; shares ISO 291 and ISO 10365) |
| ISO 9653 | shear impact strength of adhesive bonds (pendulum, 3.4 m/s; the shear-mode counterpart) |
| ASTM D950 | impact strength of adhesive bonds (the usual North-American companion in impact test plans) |
| ISO 6922 | Adhesives; Determination of tensile strength of butt joints |
| ASTM D3762 | the "Boeing wedge test": also wedge-driven, but a slow, hot/wet durability crack-growth test, not an impact test — do not confuse the two |
Test Applications:
Automotive (primary driver): body-in-white, hem-flange bonds, crash-resistant/impact-toughened structural adhesives, multi-material (steel–Al–CFRP) joints. Typically screened between −40 °C and +80 °C to cover service climate.
E-mobility: EV battery-pack bonding, where the adhesive must survive both impact and thermal duty.
Rail & transport: the Chinese national adoption was drafted with rail vehicle manufacturers involved.
Aerospace, marine, wind energy, construction: any bonded joint exposed to high-rate opening loads.
Adhesive producers & OEM QC: R&D screening of formulations and surface treatments, batch release/quality control against baseline impact data, and failure-mode (cohesive vs. interfacial) analysis.
Keywords: ISO 11343 wedge impact tester, adhesive dynamic cleavage test, structural adhesive impact cleavage resistance, wedge impact method tester, high strength adhesive bond impact test, crash rate cleavage test, automotive structural adhesive testing, composite bonded joint impact test, dynamic cleavage energy measurement, adhesive wedge impact test machine, UnitedTest adhesive mechanical testing equipment
Related products and device
Related Standard
ASTM D1822 Tensile Impact Energy to Break Plastics and Electrical Insulating Materials
ASTM D1822 standard outlines test procedures to find the energy required to rupture tension-impact specimens of plastic or electrical insulating materials. Test materials that are too bendable or too thin to be tested in accordance with the ASTM D256 standard are ideal for this test along with more rigid materials.
The ISO 5832 family is a set of material‑specification standards developed by ISO/TC 150/SC 1 (Surgical Implants‑Materials) for raw metallic materials used to manufacture surgical/orthopaedic implants. Each part defines one material grade (stainless steel, pure titanium, titanium‑alloys, cobalt‑base alloys), covering chemical composition, microstructure, mechanical requirements and test methods. All parts share highly‑aligned structural frameworks and adopt the same general mechanical‑testing rules.
ISO 11343 Wedge‑Impact Cleavage Test FAQs
A1. What is the ISO 11343 test in plain language?
ISO 11343 is an impact wedge-peel (cleavage) test for structural adhesives. Two strips of sheet material (metal or fibre-reinforced plastic) are bonded together. A hardened-steel wedge is driven at high speed into the bondline, forcing the joint open. The machine records force versus time (or versus displacement) during the few-millisecond event, and from that curve you obtain the force and the energy needed to initiate and propagate a cleavage crack.
A2. What does ISO 11343 actually measure?
Quantity | Definition | Unit |
|---|---|---|
Dynamic resistance to cleavage | Force per unit width needed to bring the joint to failure by wedge cleaving | kN/m |
Cracking force | Maximum force after which force falls to a plateau — marks crack initiation; usually the peak force | N |
Cleavage force | Momentary force during stable crack growth | N |
Average cleavage force | Mean force over the plateau, taken between the first 25 % and the last 10 % of the curve | N |
Dynamic cleavage energy | Energy needed to bring the joint to failure by wedge separation |
A3. Which industries use ISO 11343?
Primarily automotive (body-in-white, crash-resistant structural adhesives, hem-flange bonding, multi-material steel/Al/CFRP joints), then e-mobility (EV battery-pack bonding), rail and transport, aerospace, marine, wind energy, and construction. It is used both by adhesive formulators (R&D screening) and by OEMs/labs (batch QC and incoming inspection).
A4. Why is this test important for the material?
Static tests do not predict crash behaviour. Lap shear and T-peel run at mm/min. A crash loads the bondline in milliseconds, and adhesives are strongly strain-rate sensitive — ranking by static data alone can be wrong.
It loads the joint in its weakest mode. Joints are designed to carry shear but fail by opening/peeling. ISO 11343 loads them in exactly that mode, at the relevant rate.
It measures energy, not just force. Crashworthiness is about energy absorption, so the dynamic cleavage energy and the failure pattern tell you whether the bond deforms and absorbs energy (cohesive failure — good) or pops off the substrate (interfacial failure — bad).
It interrogates the interface. It is highly discriminating for surface preparation, oil contamination, primer quality and cure state. Failure pattern must be classified per ISO 10365.
It reveals temperature sensitivity. Testing between roughly −40 °C and +80 °C exposes ductile-to-brittle transitions invisible at room temperature.
It feeds CAE. Results are used to calibrate cohesive-zone and crash finite-element models.
A5. Drop tower vs. pendulum vs. servo-hydraulic — does it matter?
Yes, for the data you can extract. A servo-hydraulic machine delivers both force–time and force–displacement. Pendulum and falling-weight machines deliver force–time; force–displacement by double integration is not necessarily valid. All three machine types are acceptable under the standard, but the type must be stated in the test report.
A6. Symmetric or asymmetric wedge — which one do I use?
Identical adherends → symmetric wedge.
Different thickness, material, yield point or modulus → asymmetric wedge, with the less influential adherend (higher modulus, higher yield point or thicker) placed on the bottom, flat side of the wedge.
For high-strength steel or FRP substrates the symmetric wedge is not always suitable; the standard recommends an asymmetric wedge with a steel substrate on the upper side (the "mixed-material approach").
With the asymmetric wedge, only the top / thinner / lower-modulus adherend is bent.
A7. Can I filter the force signal?
Yes, but carefully. Because the impact event has a strong elastic component, resonant oscillations can distort the curve. The standard permits low-pass filtering, notes that it reduces measurement accuracy, and requires the filter type and characteristics to be documented in the test report. Curves that are highly irregular must be discarded.
A8. What causes bad or invalid results?
Bondline thicker than 2 mm, or thickness variation > 5 % within a set.
Excess adhesive left where the wedge first strikes (this especially corrupts the cracking force).
Damaged, bent, scratched or dirty wedge — friction inflates measured energy. The wedge must be replaced and the test discarded.
Insufficient clamping → elongated bolt hole or adherend failure at the hole.
Undocumented bend radius, or a bend radius that differs between specimen sets.
Unfiltered or over-filtered resonant signals; irregular curves.
Comparing results obtained at different speeds, temperatures, widths or on different machine types.
A9. Which standards are related to or similar to ISO 11343?
Normative references inside the standard
ISO 291 — standard atmospheres for conditioning and testing
ISO 10365 — designation of main failure patterns
EN 13887 — surface preparation of metals and plastics before adhesive bonding
Identical regional / national adoptions
EN ISO 11343:2019, DIN EN ISO 11343:2019-10, BS EN ISO 11343:2019, I.S. EN ISO 11343:2019
GB/T 36877-2018 (China) — Determination of impact peel strength of structural adhesives — Wedge method, a modified adoption of ISO 11343:2003
Complementary / neighbouring methods
ISO 25217 — quasi-static Mode I fracture energy G_IC by DCB/TDCB (the fracture-mechanics counterpart)
ISO 9653 — shear impact strength of adhesive bonds (pendulum, 3.4 m/s — the shear-mode counterpart)
ASTM D950 — impact strength of adhesive bonds (common North American companion in impact test plans)
ISO 4587 (lap shear), ISO 11339 / ISO 8510 / ISO 4578 (T-peel and 90°/180° peel), ISO 6922 (butt tensile) — the quasi-static suite ISO 11343 supplements
ASTM D3762 — the "Boeing wedge test": also wedge-driven, but a slow, hot/wet durability crack-growth test, not an impact test. Do not confuse the two.
A10. Why do automotive OEMs specifically ask for ISO 11343?
Because impact-toughened ("crash-resistant") structural adhesives are used in safety-critical areas. In a crash, uncontrolled fracture of a bonded seam defeats the crumple-zone energy-management strategy. ISO 11343 is the standardised way to prove that a bond absorbs energy at impact rates and fails cohesively rather than debonding — and to re-prove it at the temperature extremes a vehicle actually sees.
A11. What should I look for when buying an ISO 11343 test system?
Impact energy headroom above 50 J and speed capability above 2 m/s (3 m/s is common in automotive specs).
Force measurement with a response time at least one order of magnitude faster than the event; high sampling rate (MHz-class) acquisition.
A fixture set that includes both symmetric and asymmetric wedges, the wedge support frame at 820 g ± 5 g, and grips with 8-mm bolt location.
Software that automatically locates the cracking and separation points, applies the 25 %/10 % trimming rule, and computes kN/m and J.
Optional thermostatic chamber for −40 °C to +80 °C testing.
ISO 11343 fixture compatibility with your existing drop tower or pendulum, so you don't need a dedicated machine.
A12. Why choose ISO 11343 Wedge Impact Test Machine from UnitedTest?
UnitedTest manufactures ISO 11343:2019 instrumented wedge impact test machines for measuring dynamic cleavage resistance of high‑strength structural adhesive bonds. Suitable for automotive metal, aluminum and FRP bonded joint crash‑relevant impact‑peel evaluation. Complete symmetric & asymmetric wedge fixtures, data acquisition & analysis software available.
UnitedTest is a professional manufacturer of ISO 11343:2019 wedge‑impact testing equipment for structural adhesive dynamic cleavage measurement.
Our instrumented impact test systems comply fully with ISO 11343 requirements, supporting pendulum, falling‑weight and servohydraulic high‑speed impact configurations for automotive structural adhesive R&D, material screening and quality‑control laboratories.
The test system evaluates dynamic cleavage performance of high‑strength adhesive‑bonded joints under crash‑simulated high‑velocity loading (≥ 2 m/s, ≥ 50 J impact energy). It measures cracking force, average cleavage force, dynamic resistance to cleavage (kN/m) and dynamic cleavage fracture energy for metal‑to‑metal, metal‑to‑fibre‑reinforced plastic assemblies widely used in automotive body‑in‑white manufacturing.
UnitedTest supplies full ISO 11343 accessories: hardened‑steel symmetric wedge, asymmetric wedge, wedge support frame assembly (820 g ± 5 g), specimen clamping fixtures with 8 mm locating bolt holes, high‑response force transducer and professional analysis software. The software can process force‑time / force‑displacement curves, support signal filtering and automatically compute key test parameters, generating complete test reports matching ISO 11343 reporting requirements.
Our testing solutions help adhesive manufacturers, automotive OEMs and research institutes compare different adhesive grades, substrate materials, surface pretreatment and curing processes under impact‑cleavage conditions.
Require More Customized Solutions?