Home >> Application >> By Standard >> ASTM >> ASTM D >> ASTM D751 Coated Fabric Test Method and Testing Machine

ASTM D751 Coated Fabric Test Method and Testing Machine

Share:

ASTM D751 Standard Test Methods for Coated Fabrics

ASTM D751 is an umbrella book of physical/mechanical test methods for coated fabrics, not a product specification. It covers, but is not limited to, rubber-coated fabrics such as tarpaulins, rainwear and similar products; in practice it is also widely applied to PVC-, PU- and other polymer-coated fabrics.

Its purpose is to give manufacturers, buyers and laboratories repeatable ways to measure quality: dimensions/mass, tensile and tear strength, burst and puncture resistance, coating adhesion, seam performance, water resistance, low-temperature behaviour, heat ageing, blocking, crush and wicking. It does not set pass/fail limits — acceptance criteria come from the material or product specification. 

For UnitedTest, the commercial meaning is straightforward: D751 defines a family of test machines and fixtures. Most mechanical clauses run on a constant-rate-of-extension universal testing machine (UTM) with interchangeable grips and fixtures; hydrostatic resistance, blocking, wicking, low-temperature impact and heat ageing require dedicated apparatus. One UTM supplier’s application note confirms that most D751 tests can be done on a UTM with dedicated grips, while hydrostatic, blocking, wicking and impact equipment are separate systems.


ASTM D751 Coated Fabric Test Method and Testing Machine


Master index — every method at a glance

Method / procedureMeasuresCore equipmentUnitedTest product family
Dimensions & MassLength, width, thickness, mass/areaMeasuring drum, deadweight thickness gauge, 0.25 % scaleDimensional gauges, balances
Breaking Strength A — GrabMax tensile force, MD/XMDUTM + 25/50 mm grab jawsUTM 5–10 kN
Breaking Strength B — Cut StripMax force on 25 mm stripSame UTM + strip cutting dieUTM + dies
Elongation% elongation at stated forceSame UTM + elongation recorderUTM software
Bursting A — Ball BurstForce to burst by steel ballUTM + 44.45 mm ring clamp + 25.40 mm ballBurst fixture
Bursting B — Diaphragm BurstHydraulic bursting pressureMullen/diaphragm tester, 31 mm apertureHydraulic burst tester
Puncture ResistanceForce to penetrateSame ring clamp + flat-tip probePuncture fixture
Tearing A — PendulumElmendorf tear energyFalling-pendulum tear testerStand-alone Elmendorf
Tearing B — Tongue TearTear propagation forceUTM + 25×50 mm jawsUTM 500 N–1 kN
Trapezoidal TearTear force on trapezoidSame UTM, 25 mm gauge, templateUTM + cutting die
Hydrostatic A — MullenWater penetration pressureMullen-type hydrostatic testerHydrostatic tester
Hydrostatic B — Rising ColumnWater column height / time-to-leakSuter rising-water-column apparatusHydrostatic head tester
Coating Adhesion (Peel)Bond strength N/25 mmUTM + 25×76 mm peel jawsUTM + peel fixture
Strength of CoatingCoating durability after pre-tensioningUTM with load-hold + hydrostatic testerUTM + hydrostatic
Tack-Tear ResistanceTear at tacked needlesFig. 4 needle fixture + UTMCustom tack-tear rig
Low-Temp BendCold flexibility, pass/failChamber + bend fixture to D2136Low-temp chamber
Low-Temp ImpactBrittleness pointD2137 impact testerBrittleness tester
Low-Temp Crack ResistanceCold crease + retained hydrostaticCold chamber + 4.5 kg roller + hydrostatic BChamber + hydrostatic
Seam StrengthSeam vs fabric strengthUTM + 25×76 mm jawsUTM
Accelerated Heat Aging% property change after oven ageingAir oven to D573Aging oven
Dead Load Seam StrengthSustained-load seam integrityConstant-load frame + ovenCreep / dead-load frame
Blocking ResistanceSurface sticking at heatGlass plates + 1.8 kg + ovenBlocking oven
Crush ResistanceLocalized crush/cut forceCompression machine + Fig. 5/6 buttonCompression tester ≥ 5.3 kN
WickingDye-wicking lengthBeaker, dye, magnifierWicking station


Details guide of ASTM D751 Coated Fabric Test Method and Testing Machine

Recommend UnitedTest Universal Testing Machine and related test fixtures. 

1. Breaking Strength 

(Grab Test + Cut Strip Test)

Measures the maximum tensile force a coated fabric can sustain before rupture, tested separately in warp (longitudinal) and fill (transverse) directions.

  • Universal tensile testing machine with constant-speed straining mechanism

  • Specimen clamps with flat, parallel gripping surfaces (edges rounded to prevent cutting damage)

  • Specimen Information

    Grab test: 102 mm (4 in.) wide × ≥152 mm (6 in.) long; 5 specimens per direction

    Cut strip test: 25 mm (1 in.) wide strips, same length requirement

2. Bursting Strength 

(Ball Burst Method + Diaphragm Burst Method)

Evaluates resistance to multi-directional rupture when pressure is applied perpendicular to the fabric surface, simulating inflation, impact or distributed load conditions.

  • Procedure A – Ball Burst: Universal tensile machine + ring-clamp fixture (44.45 ± 0.05 mm inner diameter) + polished steel ball (25.40 ± 0.05 mm diameter)

  • Procedure B – Diaphragm Burst: Hydraulic bursting tester with annular coaxial clamps (31.0 ± 0.8 mm aperture), rubber diaphragm, Bourdon pressure gauge, piston-driven hydraulic system

Ball burst: crosshead speed 5.0 ± 0.2 mm/s; load resolution 5 N (1 lbf)

Specimen Information

Ball burst: ≥5 specimens; minimum dimension 12 mm larger than clamp outer diameter

Diaphragm burst: ≥10 specimens; 125 mm (5 in.) square or circular

3. Puncture Resistance

Measures the peak force required to fully pierce a coated fabric with a defined sharp probe, simulating puncture damage from sharp objects in service.

Test Equipment: Same universal tensile machine and ring clamp used for ball burst testing, with the steel ball replaced by a specialized flat-tip flared piercing probe.

  • Probe tip dimensions: 7.92 ± 2.5 mm width, 0.8 ± 0.1 mm thickness, edges rounded to 0.25 mm radius

  • Probe orientation: approximately 45° to warp and fill yarns

  • Test speed: 5.0 ± 0.2 mm/s

Specimen Information: 5 circular specimens; diameter at least 12.7 mm (0.5 in.) larger than the clamp outer diameter.

4. Tearing Strength (3 Methods)

Quantifies resistance to tear propagation under three different loading modes: pendulum impact tear, static tongue tear and trapezoidal tear.

  • Procedure A – Pendulum Method: Elmendorf-type falling pendulum tester

  • Procedure B – Tongue Tear Method: Universal tensile machine with 25 × 50 mm jaw faces

  • Trapezoidal Tear: Universal tensile machine with 25 × 50 mm jaws + trapezoid marking template

5. Seam Strength 

Determines the tensile strength of lapped, bonded and sewn seams, for direct comparison to the base fabric breaking strength.

Universal tensile machine (same platform as grab breaking strength) with modified jaws: minimum 25 × 76 mm (1 × 3 in.) face dimensions.

6. Crush Resistance

Evaluates resistance to crushing and cutting under concentrated compressive load, developed specifically for coated-fabric diaphragm materials used in automotive and regulator devices.

  • Compression testing machine (or universal machine in compression mode)

  • Flat base plate

  • Load button assembly (defined geometry with 45° chamfer and 1.5 mm radius tip)

7. Tack-Tear Resistance

Simulates tearing damage when coated fabric is tacked (nailed or stapled) in place, primarily for vinyl upholstery and automotive interior fabrics.

  • Universal tensile machine

  • Specialized tack-tear fixture with a line of needles (detailed dimensions defined in the standard)


Specimen: 50 mm (2 in.) wide × 152 mm (6 in.) long; 5 specimens each for warp and fill directions.

8. Accelerated Heat Aging

Estimates the relative heat deterioration resistance of rubber- or plastic-coated fabrics by measuring retention of mechanical properties after controlled elevated-temperature air exposure.

  • Circulating air oven conforming to ASTM D573

  • Standard test equipment for the target properties (breaking strength, burst strength, tear strength, etc.)

9, Low-Temperature Performance Tests

Pass/fail flexibility of coated fabric at a specified low temperature.

Equipment. Low-temperature chamber/bath and bend fixture to ASTM D2136; D751 delegates entirely.

10. Blocking Resistance at Elevated TemperaturesDetermines whether coated fabric surfaces adhere to each other ("block") when stacked under pressure at elevated temperatures — a critical property for rolled storage and high-temperature service.
Other test

Dimensions and Mass;

Hydrostatic Resistance;

Adhesion of Coating to Fabric (Peel Test);

Strength of Coating;

Dead Load Seam Strength;

Wicking of Coated Cloth.


Related Standard:

ASTM D751
Standard Test Methods for Coated Fabrics
ASTM D573Standard Test Method for Rubber—Deterioration in an Air Oven
ASTM D1424

Elmendorf pendulum tear

ASTM D2136Standard Test Method for Coated Fabrics—Low-Temperature Bend Test
ASTM D2137brittleness point / low-temperature impact
ISO 1421Rubber- or plastics-coated fabrics - Determination of tensile strength and elongation at break
ISO 2411Rubber- or plastics-coated fabrics — Determination of coating adhesion
ISO 4674-1Rubber- or plastics-coated fabrics - Determination of tear resistance - Part 1: Constant rate of tear methods
ASTM D3393Standard Specification for Coated Fabrics—Waterproofness
ASTM D5034Test Method for Breaking Strength and Elongation of Textile Fabrics (Grab Test).
ASTM D5035Test Method for Breaking Force and Elongation of Textile Fabrics (Strip Method)
ASTM D3786Bursting Strength of Textile Fabrics—Diaphragm Bursting Strength Tester Method
ASTM D3787Test Method for Bursting Strength of Textiles&x2014;Constant-Rate-of-Traverse (CRT) Ball Burst Test


Keywords: ASTM D751, ASTM D751 test methods, coated fabric testing, rubber coated fabric test standard, coated fabric testing machine, ASTM D751 testing equipment, breaking strength tester, bursting strength tester, tear strength tester, hydrostatic resistance tester, peel adhesion test, low temperature bend test, heat aging oven, grab test method, ball burst method, diaphragm burst test, tongue tear test, trapezoidal tear, tack-tear resistance, crush resistance tester, seam strength test, UnitedTest

Related products and device

ASTM D751 Coated Fabric Universal Testing machine

WDW Series Computer Control Electronic Universal Testing Machine made by UNITEDTEST range from 100N to 600KN load capacity with various models like single columns, table type, door frame type etc., is used to perform tension, compression, flexure/bending, shearing, peeling etc., test for metal and nonmetal specimens. Matched with UNITEDTEST design and produced various test fixture, like peel, flexure, puncture, tear, pneumatic grip, belt tension etc., this UTM can be used to almost all materials include but not limited to steel rod, rubber, steel wire, plastic, seat belt, textile, wood, panel etc., mechanical performance inspection.

ASTM D751 Coated Fabric tear strength tester, peel adhesion test

A single column tensile tester is a sophisticated material testing instrument designed for measuring mechanical properties of various materials under tension, compression, bending, shear, and other loading conditions. As the name suggests, it features a single vertical column supporting a moving crosshead that applies force to test specimens.

ASTM D751 test equipment, Coated Fabric material flexural test instrument

Three-point bending test fixture for fiber-reinforced plastic composites, designed in accordance with ISO 14125, provides a standardized method for determining the flexural properties of composite materials using a three-point bending test.

ASTM D751 Electricity hot blast drying oven

Electricity hot blast drying oven is mainly used to measure the dimension change of plastic material after heating, suitable for plastic pipe, plastic sheet etc.

ASTM D751 Large Scale Hydrostatic Puncture Testing Machine

Geosynthetic membrane hydrostatic pressure testing instrument is a specialized device used to detect the static water pressure resistance of non-woven composite geosynthetic membranes.

Related Standard

ISO 5470-2 Martindale Abrasion Test for Rubber or Plastics-Coated Fabrics –

ISO 5470-2 — Rubber- or plastics-coated fabrics — Determination of abrasion resistance — Part 2: Martindale abrader

ISO 5470-2 specifying laboratory abrasion‑resistance evaluation for coated fabrics using a Martindale‑type tester, covering both dry‑abrasion and wet‑abrasion test conditions. It is used for quality control, product development and coating-formulation comparison, type approval, and contractual specification compliance.

ASTM F3152 abrasion test for inks and coatings –

ASTM F3152 Standard Test Method for Determining Abrasion Resistance of Inks and Coatings on Substrates Using Dry or Wet Abrasive Medium

ASTM F3152 evaluating abrasion resistance of surface‑printed inks and coatings on substrates, supporting both dry‑abrasion and wet‑abrasion modes with optional chemical exposure.

ASTM F2357 Abrasion Resistance Testing for Inks, Coatings & Membrane Switches –

ASTM F2357 Standard Test Method for Determining the Abrasion Resistance of Inks and Coatings on Membrane Switches Using the Norman Tool "RCA" Abrader

ASTM F2357 defines a comparative, accelerated abrasion test in which a strip of abrasive paper (or polyester tape) is drawn repeatedly across the printed or coated surface of a membrane switch under a specified normal load, and the surface is inspected at intervals until a defined visual failure point is reached. The result is reported as the number of cycles to "wear limit" and to "final breakthrough." It is explicitly a relative ranking tool — not a predictor of service life in finger-touches.

EN 1719 Loop tack measurement for coated pressure-sensitive adhesives –

EN 1719 specifies test method to quantify the loop tack of coated pressure-sensitive adhesives (PSAs)—a critical property for adhesives used in applications requiring rapid, low pressure, initial bonding (e.g., labels, tapes, disposable hygiene products). The standard aligns with European Committee for Standardization (CEN) requirements and is intended for quality control, research, and regulatory compliance in the adhesive and packaging industries. 

ASTM F1160 Shear and Bending Fatigue testing of Coatings for Calcium Phosphate and Metallic –

ASTM F1160 Standard Test Method for Shear and Bending Fatigue Testing of Calcium Phosphate and Metallic Medical and Composite Calcium Phosphate/Metallic Coatings;


Rotating beam fatigue testing generates higher frequencies than traditional high cycle fatigue (HCF) methods. UnitedTest testing services provide critical data about coatings and metallic surface treatments to ISO 1143, ASTM F1160 standards. 


Rotating beam fatigue testing, Shear and Bending Fatigue testing. 

Rotating beam fatigue testing is a mechanical test method used to evaluate the fatigue properties of materials. In this test, a beam specimen is subjected to cyclic loading, which induces repeated bending causing failure over time. The specimen is mounted on a rotating apparatus, which allows for the cyclic load to be applied at constant amplitude and frequency.

During the test, the beam specimen is rotated at a constant speed while a loading force is applied to it. The force causes the beam to bend, and as the beam rotates, it undergoes cyclic bending stress that can induce fatigue failure.

ISO 5470-1 Abrasion Test of Rubber or Plastics Coated Fabrics by Taber Abrader Method –

ISO 5470-1: Rubber- or plastics-coated fabrics -- Determination of abrasion resistance -- Part 1: Taber abrader.

ISO 5470-1 specifies a method for determining the abrasion resistance of rubber- or plastics-coated fabrics using the Taber abrader apparatus. This test simulates wear under controlled conditions to evaluate a material's durability.

Frequently Asked Questions About ASTM D751 Coated Fabric Test Method and Testing Machine

Q1. What is ASTM D751 used for?

ASTM D751, Standard Test Methods for Coated Fabrics, is the umbrella test-method standard used to measure the physical and mechanical quality of rubber-, PVC- and PU-coated fabrics — tarpaulins, rainwear, truck covers, architectural membranes and similar products. It covers dimensions and mass, breaking strength, elongation, bursting strength, puncture resistance, tearing strength, hydrostatic resistance, coating adhesion, seam strength, low-temperature behaviour, heat ageing, blocking, crush resistance and wicking. It is a test-method standard, not a product specification: it tells a lab how to test, while the material or buyer specification sets the pass/fail limit. SI units are the standard; inch-pound values in parentheses are informational only.


Q2. What testing machine is required for ASTM D751?

The baseline is a constant-rate-of-extension universal testing machine (UTM) per Section 12: a straining mechanism, specimen clamps, and a load/elongation recording system that holds the maximum load after rupture. Key specs: 5 ± 0.2 mm/s (300 mm/min, 12 ± 0.5 in/min), use 15–85 % of rated capacity, force error ≤ 2 % up to 222 N and ≤ 1 % above 222 N, and a 75 mm (3 in.) initial clamp separation with 25 mm gripping surfaces in the load direction. Dedicated instruments are additionally needed for hydrostatic resistance, pendulum tear, heat ageing, blocking, low-temperature impact and wicking.


Q3. Can one universal testing machine cover all ASTM D751 mechanical tests?

Yes — one UTM frame covers most of the mechanical clauses when fitted with the right grips and fixtures: grab, cut strip, elongation, ball burst, puncture, tongue tear, trapezoidal tear, peel adhesion, tack-tear, seam strength, dead-load seam, coating pre-tensioning and crush resistance. It does not replace a Mullen/rising-column hydrostatic tester, an Elmendorf pendulum tear tester, an air-oven ageing chamber, a low-temperature brittleness tester, a blocking oven or a wicking station. A modular ASTM D751 fixture kit is therefore the most credible product offer: one frame, a low-force and a high-force load cell, and certified interchangeable jaws.


Q4. What load cell size do I need for ASTM D751 grab test vs tear and peel test?

Size for two very different force ranges. Heavy PVC tarpaulin grab strength typically falls around 1.5–6 kN, so a 5–10 kN frame with a 5 kN load cell covers ASTM D751 grab and cut-strip work. Tear, peel adhesion and seam peaks are commonly 20–500 N, where a 500 N or 1 kN cell keeps readings in the accurate part of the range and satisfies the 15–85 % capacity rule. Offering a dual-load-cell ASTM D751 testing machine removes the most common buying objection.


Q5. Is there an "ASTM-certified" D751 testing machine?

No. ASTM International develops standards; it does not approve, certify or endorse testing instruments. The accurate wording is "testing machine configured to ASTM D751 requirements", "designed for ASTM D751 test methods", or "ASTM D751-compliant fixture geometry". What you should supply instead is traceable force, displacement, speed, pressure and temperature calibration certificates, plus a fixture dimension report against Figs. 1–6. Avoid "ASTM approved" in titles and ads — it is a compliance risk and a trust signal loss.


Q6. Which ASTM D751 fixtures and grips should a supplier quote?

Minimum kit: 25 × 25 mm front / 25 × ≥ 50 mm rear grab jaws; 25 mm strip cutting die; 44.45 ± 0.05 mm ID ring clamp + 25.40 ± 0.05 mm polished steel ball for ball burst; 7.92 mm flat-tip screwdriver probe for puncture; 25 × 50 mm tongue/trapezoid jaws; 25 × 76 mm peel and seam jaws; trapezoidal template with 15.9 mm cut; Fig. 4 tack-tear needle fixture; Fig. 5 base plate and Fig. 6 load button for crush; plus certified specimen cutting dies. Edge radii ≤ 0.4 mm and jaw flatness/parallelism (carbon-paper check, Note 4) are small details that win lab audits.


Q7. What machine is needed for ASTM D751 crush resistance?

Sections 94–98 require a compression testing machine at 0.084 mm/s (0.0033 in/s ≈ 5 mm/min), capacity ≥ 5338 N (1200 lbf), accuracy ≤ 2 % ≤ 222 N and ≤ 1 % above, with the Fig. 5 base plate and Fig. 6 load-button assembly. Test ≥ 50 × 203 mm specimens, place the button ≥ 12.7 mm from any edge and from prior test areas, run at least three areas, and record the force at crush/cut. Note 11: for unbalanced coatings, the thicker coating side faces upward. Report force, conditioning period and post-test coating condition.


Q8. How does ASTM D751 blocking resistance differ from ISO 5978?

D751 (89–93) uses three 203 × 203 mm specimens folded face-to-face then back-to-back into 102 × 102 mm, between two ~100 × 100 × 3 mm glass plates under 1.8 kg, default 6 h at 66 ± 1 °C, ≥ 5 min cooling, then a 1 / 2 / 3 rating (no blocking / slight blocking / blocking). ISO 5978:2023 uses 150 ± 2 mm specimens, 70 ± 2 °C for 3 h, ≈ 2.18 kPa and ≥ 6 air changes per hour. Same oven family, different parameters — never claim one certificate covers both.


Q9. What does the ASTM D751 accelerated heat aging test involve?

Sections 77–84 use an air oven conforming to ASTM D573 apparatus, preheated, with specimens strain-free, freely exposed on all sides and unlit. Temperature comes from D1349; typical intervals are 1, 2, 3, 7 days or multiples of 7; use ≥ 3 specimens for original and aged properties. Measure breaking strength, burst strength, tear strength or other properties before and after, then report percent change c = (A − O)/O × 100. The standard is explicit: results are comparative only, with no exact correlation to natural service life.


Q10. Which ASTM D751 low-temperature tests require separate chambers?

Three. Section 64 (low-temperature bend) delegates entirely to ASTM D2136 — a pass/fail 180° bend at a specified cold temperature. Section 65 (low-temperature impact) delegates to ASTM D2137, requiring a cantilever clamp and a 2.0 ± 0.2 m/s striker in a cooled chamber/bath. Sections 66–70 (low-temperature crack resistance) use a 203 mm square specimen, ≥ 3 per lot, a 4.5 kg steel roller (~140 mm diameter × 51 mm wide) for a single 180° crease in warp and fill, visual crack inspection, ≥ 2 h return to standard conditions, then Procedure B hydrostatic verification. That is a chamber + roller + hydrostatic tester bundle, not a UTM accessory.


Q11. ASTM D751 grab test vs cut strip test — what is the difference, and how does it compare with ISO 1421?

Procedure A (grab) uses a 102 mm × ≥ 152 mm specimen gripped across a 25 mm central jaw area; Procedure B (cut strip) uses a 25 mm wide strip cut to contain 25 mm of yarn. Both run at 5 ± 0.2 mm/s, use two sets of five specimens in MD/XMD, and report the average per direction — but the results are not interchangeable, because the effective tested width differs. Also note ISO 1421 runs at 100 mm/min, while ASTM D751 runs at 300 mm/min; never cross-quote D751 and ISO 1421 tensile values in one certificate.


Q12. ASTM D751 ball burst vs diaphragm burst — which tester do I need?

Procedure A (ball burst) is a UTM force test: 44.45 mm ring clamp, 25.40 mm polished steel ball, 5.0 ± 0.2 mm/s, ≥ 5 specimens, maximum force recorded to the nearest 5 N. Procedure B (diaphragm burst) is a hydraulic pressure test: 31.0 ± 0.8 mm coaxial aperture, rubber diaphragm, piston displacement 95 ± 5 mL/min, 10 specimens, result in kPa = total pressure − tare diaphragm pressure; hand-driven units run the wheel at 120 rpm. They are two different instruments, and D751 Annex A1 Table A1.5 gives precision data only for the diaphragm method.


Q13. What are the ASTM D751 puncture probe dimensions?

Section 27 replaces the ball with a flared, flat-tip screwdriver-shaped probe: width 7.92 ± 2.5 mm (0.312 ± 0.1 in.), tip thickness 0.8 ± 0.1 mm (0.031 ± 0.004 in.), tip edges rounded to a 0.25 mm (0.01 in.) radius, oriented at approximately 45° to warp and fill. Five circular specimens (diameter ≥ ring-clamp OD + 12.7 mm) are penetrated at 5.0 ± 0.2 mm/s; report the arithmetic mean in N or lbf. The probe reuses the ball-burst ring clamp, so it is a low-cost add-on fixture.


Q14. Which ASTM D751 tear test method should we build for?

There are three. Procedure A — pendulum is performed entirely to ASTM D1424 on a stand-alone Elmendorf tester. Procedure B — tongue tear uses a 76 × 203 mm specimen with a 76 mm central cut, 5 warp + 5 fill, 25 × 50 mm jaws, and 0.85 ± 0.04 mm/s or 5.00 ± 0.2 mm/s; report the average of the five highest peaks excluding the initial peak, to 0.4 N. Trapezoidal tear (Procedure C in D751-26) uses a 76 × 152 mm specimen, 25 × 102 mm trapezoid template, 15.9 mm cut, 25 ± 1 mm gauge and 5.00 ± 0.2 mm/s. Tongue tear is invalid for fabrics whose yarns bunch up before tearing.


Q15. Mullen-type vs rising water column hydrostatic tester — when is each used for ASTM D751?

Procedure A (Mullen-type, 42–45) is the default: 31.8 ± 0.5 mm apertures, grooved clamp faces, piston displacement 1.4 ± 0.1 cm³/s (≈ 85 mL/min), maximum-reading Bourdon gauge. Procedure 1 ramps pressure over 10 determinations; Procedure 2 holds a specified pressure within 14 kPa (2 psi) for 5 min on ≥ 5 specimens. Note 9: if the material gives less than 35 kPa (5 psi), switch to Procedure B, the rising-water-column (Suter) apparatus with a ≥ 203 mm square specimen, 10 mm/s column rise and reading to 1.6 mm. Procedure B is also reused by coating-strength and low-temperature crack-resistance testing.


Q16. How is ASTM D751 coating adhesion tested and reported?

Peel adhesion uses a 25 × 203 mm specimen on a UTM at 0.85 ± 0.04 mm/s or 5.00 ± 0.2 mm/s, with 25 × 76 mm jaws, 25 mm initial separation and ≥ 76 mm of peel. Report in N/25 mm (lbf/1 in.) as the average of the five highest peaks excluding the initial peak; the five low peaks may be reported for peel range. Test longitudinal and transverse directions, and both sides if double-coated. Editorial caution: D751-19 §51.1 gives conflicting specimen counts ("two sets of three" then "two sets of two"), while §53.1.2 requires at least three per direction — design for ≥ 3 per direction and verify against D751-26. ISO 2411 is the international counterpart.


Q17. What is the difference between ASTM D751 seam strength and dead load seam strength?

Seam strength (71–76) is a short-term modified grab pull: 50 × 203 mm specimen, seam centred horizontally, 25 × 76 mm jaws, 5.00 ± 0.2 mm/s, three specimens, reported in N/25 mm with a mandatory note on whether failure occurred in the seam or in the fabric. Dead load seam strength (85–88) is a sustained-load/creep test: 25 ± 0.5 mm wide strip with 76 mm on each side of the seam, clamps within 1 in. of the seam edge, constant load held to ± 1 %, optional circulating-air oven within ± 2 °F, three specimens, pass/fail — failure of any specimen fails the test. Different machines, different selling points.


Q18. Does ASTM D751 include a fatigue test, UV exposure or weathering?

No. ASTM D751 has no high-cycle dynamic fatigue machine and no light-exposure chamber — Section 78.1 explicitly says oven ageing "does not include exposure to light". The closest D751 clauses are dead load seam strength (static creep), strength of coating (load-hold preconditioning to 133.5 ± 4.5 N for 30 s), accelerated heat aging (77–84), low-temperature crack resistance (66–70) and blocking resistance (89–93). For cyclic flex fatigue, point customers to ISO 7854 / DIN 53359; for UV/weathering, to ISO 4892-2 / ASTM G154; for flame, to ASTM D6413 / NFPA 701. D751 also does not cover air permeability, mildew resistance or fibre content.

< Previous: ASTM D746 Impact Test for Brittleness Temperature of Plastics and Elastomers

> Next: ASTM D790 Bending Test Flexural Properties of Unreinforced and Reinforced Plastics

Require More Customized Solutions?

We offer customization to meet your specific needs. Our expert team will collaborate with you to develop the perfect product for you
Customize Now

Beijing United Test Co., Ltd.