Home >> Application >> By Standard >> ISO >> ISO 5000~9999 >> ISO 5832 Tensile Testing for Surgical Implant Metals

ISO 5832 Tensile Testing for Surgical Implant Metals

Share:

The ISO 5832 family is a set of material‑specification standards developed by ISO/TC 150/SC 1 (Surgical Implants‑Materials) for raw metallic materials used to manufacture surgical/orthopaedic implants. Each part defines one material grade (stainless steel, pure titanium, titanium‑alloys, cobalt‑base alloys), covering chemical composition, microstructure, mechanical requirements and test methods. All parts share highly‑aligned structural frameworks and adopt the same general mechanical‑testing rules.


ISO 6892‑1: Fundamental test‑method standard: defines how to run tensile test, machine, specimen, calculation.

ISO 5832 Tensile Testing for Surgical Implant Metals


Main parts overview

Standard No.Material
ISO 5832‑1:2024Wrought stainless steel (S31673)
ISO 5832‑2:2018Unalloyed titanium (commercially pure Ti grades 1‑4B)
ISO 5832‑3:2021Wrought Ti‑6Al‑4V alloy (including ELI grade)
ISO 5832‑4:2024Cast Co‑Cr‑Mo alloy (cast implant alloy)
ISO 5832‑5:2022Wrought Co‑Cr‑W‑Ni alloy
ISO 5832‑6:2022Wrought Co‑Ni‑Cr‑Mo alloy
ISO 5832‑7:2024Forgeable & cold‑formed Co‑Cr‑Ni‑Mo‑Fe alloy
ISO 5832‑8:1997Wrought Co‑Ni‑Cr‑Mo‑W‑Fe alloy
ISO 5832‑9:2019Wrought high‑nitrogen stainless steel
ISO 5832‑11:2024Wrought Ti‑6Al‑7Nb alloy
ISO 5832‑14:2019Wrought Ti‑15Mo‑5Zr‑3Al (beta‑titanium) alloy


Test Equipment required for ISO 5832 Tensile Testing for Surgical Implant Metals

Universal testing machine    

Machine type: Computer‑controlled universal tensile testing machine (UTM), performing uniaxial tension at room‑temperature environment (ambient 10 ~ 35 °C).

Force‑measurement system: Load‑cell must meet accuracy class 1 or better, with valid traceable calibration certificate. Force range must cover expected breaking load of specimens.

Strain‑measuring device: Extensometer (clip‑on contact‑type or non‑contact video‑extensometer) for measuring yield strength Rp0.2. Extensometer shall meet corresponding accuracy grade for strain measurement.

Control: Capable of constant strain‑rate / constant stress‑rate control mode; test speed shall comply with ISO 6892‑1 provisions (different speed ranges for yield region and post‑yield region).

Calibration: Periodic verification of force, displacement and strain channels as per national metrology requirements.

Gripping system

Suitable fixtures for bar, wire, sheet/strip specimens to prevent slipping and eccentric loading.

A ISO 5832 tensile testing machine is a universal testing machine configured to qualify the metallic raw materials used to manufacture surgical implants — stainless steel, unalloyed titanium, Ti-6Al-4V, Ti-6Al-7Nb, Ti-15Mo-5Zr-3Al and the cobalt-chromium alloy family. UnitedTest builds and calibrates these systems to the accuracy classes the standards actually demand: ISO 7500-1 class 0.5 for the force system, ISO 9513 class 0.5 for the extensometer, and true closed-loop ISO 6892-1 Method A strain-rate control.


Measured tensile parameters required by ISO 5832:

Each material part defines minimum/mandatory values for these tensile indexes in material‑condition tables (annealed / hot‑worked / cold‑worked / cold‑drawn etc.):

  1. Rm: Tensile strength (MPa, minimum value)

  2. Rp0.2: 0.2 % proof / yield strength (MPa, minimum value)

  3. A: Percentage elongation after fracture (%)

  4. Z: Percentage reduction of area (%) (specified for some titanium‑alloy grades)


Property limits your customers are testing against

ISO 5832 partMaterialConditionRm (MPa)Rp0.2 (MPa)A (%)
-2Unalloyed Ti, Grade 4AAnnealed55048315
-3Ti-6Al-4V, barAnnealed86078010
-11Ti-6Al-7Nb, barAnnealed90080010
-14Ti-15Mo-5Zr-3Al, barSolution annealed90080012
-4Co-Cr-Mo, castingAs specified6654508
-12Wrought Co-Cr-MoWarm worked117282712
-6Co-Ni-Cr-MoHard1207100010
-7Co-Cr-Ni-Mo-FeSpring temper165014001
-1Wrought stainless steel, barCold worked860–110069012
-9High-N stainless, barAnnealed74043035

Minimum values unless a range is shown. Parts 2 and 11 also require reduction of area Z. Full tables for every condition are in the UnitedTest ISO 5832 application guide.


Industry Application Fields

Adhesive manufacturers: development and batch QC of PVAc, urea-formaldehyde, phenol-resorcinol, epoxy, polyurethane, hot-melt, etc. for wood bonding.

Wood products and joinery: furniture, cabinets, carpentry, flooring adhesives.

Engineered wood and timber engineering laboratories: screening adhesives before structural-grade qualification, though structural performance often requires additional standards.

Research institutes and third-party testing labs: comparative benchmarking, failure analysis, supplier qualification.

Standards/regulatory work: generating reproducible shear data for specifications and acceptance.


Related Stadard: 

PartASTMUNSEN / BS / DINJISChina
-1F138 (bar/wire), F139 (sheet/strip)S31673EN ISO 5832-1—GB 4234.1
-2F67R50250…R50700EN ISO 5832-2JIS T 7401-1GB/T 13810
-3F1472 (std), F136 (ELI)R56400/401EN ISO 5832-3:2021JIS T 7401-2GB/T 13810 (TC4)
-4F75R30075EN ISO 5832-4—GB 4234.4 / GB 17100
-5F90 (L-605)R30605EN ISO 5832-5—YY/T 0605.5
-6F562 (MP35N)R30035EN ISO 5832-6—YY/T 0605.6
-7F1058 (Elgiloy/Phynox)R30003/8EN ISO 5832-7 (also AMS 5833)—YY/T 0605.7
-8F563 (withdrawn 2005)R30563EN ISO 5832-8—YY/T 0605.8
-9F1586S31675EN ISO 5832-9—YY 0605.9 / GB 4234.9
-11F1295R56700EN ISO 5832-11JIS T 7401-5GB 23102 → GB 4234.11
-12F1537R31537/8/9EN ISO 5832-12—YY 0605.12
-14no direct ASTM (Japanese-origin β alloy)—EN ISO 5832-14 / BS ISO 5832-14JIS T 7401 seriesGB/T 4234.14*

Other auxiliary referenced standards:

ISO 6892‑1: Fundamental test‑method standard: defines how to run tensile test, machine, specimen, calculation.

- ISO 377: Sampling location & specimen preparation for steel products

- ISO 7438: Metallic materials‑Bend test (for sheet/strip bend requirement)


Keywords: ISO 5832 tensile testing machine, ISO 5832 universal testing machine, implant material tensile testing machine, medical implant metal testing equipment, ISO 6892-1 tensile testing machine, surgical implant metallic materials testing, Ti-6Al-4V tensile test machine (ISO 5832-3), Ti-6Al-7Nb tensile testing (ISO 5832-11), CoCrMo wrought alloy tensile testing (ISO 5832-12), cobalt chromium casting alloy testing (ISO 5832-4), unalloyed titanium tensile test (ISO 5832-2), implant stainless steel wire tensile tester (ISO 5832-1), high nitrogen stainless steel testing (ISO 5832-9), ISO 7438 bend test machine titanium sheet, ISO 7500-1 class 0.5 testing machine, ISO 9513 class 1 extensometer tensile, Rp0.2 proof strength testing machine

Related products and device

ISO 5832 Tensile Testing for Surgical Implant Metals

A single column tensile tester is a sophisticated material testing instrument designed for measuring mechanical properties of various materials under tension, compression, bending, shear, and other loading conditions. As the name suggests, it features a single vertical column supporting a moving crosshead that applies force to test specimens.

ISO 6238 block shear specimen wood glue strength test rig

UnitedTest manufactures and exports compressive shear test fixtures, ISO 6238 wood adhesive shear jigs, ASTM D905 block shear fixtures, ASTM D4501 rigid‑substrate shear tools, and compatible universal testing machines. Buy ISO 6238 and ASTM D905 compressive shear test fixtures from UnitedTest.

ISO 6237 Shear methods tensile test fixture

Vice Tensile test fixture for plastics is based on the test standatd ASTM D638, determination of the tensile properties of unreinforced and reinforced plastics in the form of standard dumbbell-shaped test specimens when tested under defined conditions of pretreatment, temperature, speed.

Related Standard

ISO 6892-1 Metallic materials - Tensile testing –

ISO 6892 specifies the method for tensile testing of metallic materials and defines the mechanical properties which can be determined at room temperature.  Related standard ASTM E8 , JIS Z2241 Method of tensile test for metallic materials.

ISO 7438 Metallic materials Bending test details –

ISO 7438 is a standard that specifies a method for determining the ability of metallic materials to undergo plastic deformation in bending. It is used to evaluate the flexural strength and stiffness of a material , The bend test shall be carried out in testing machines equipped with a bending device with two supports and a former; bending device with a V-block and a former; bending device with a clamp. 

ASTM F2502 Test of Internal Fixation Implants Bioabsorbable Plates and Screws –

ASTM F2502 Standard Specification and Test Methods for Absorbable Plates and Screws for Internal Fixation Implants

ASTM F2502 defines the requirements and mechanical test methods specifically for bioabsorbable (or biodegradable) orthopedic implants used to stabilize bone fractures. Unlike permanent metal implants, these devices are designed to provide temporary support and then gradually dissolve in the body. This standard ensures they possess sufficient initial mechanical strength and that their degradation properties are characterized in a standardized way. 

ASTM F2706 Fatigue Static Test of Spinal implant constructs –

ASTM F2706 is a critical biomechanical evaluation tool in the medical device industry, specifically for spinal implants. ASTM F2706 establishes standardized mechanical test methods to evaluate the static (strength) and fatigue (long-term durability) performance of spinal implant assemblies intended for use in the occipito-cervical (OC) and cervico-thoracic (CT) regions (from the skull to the upper back). It simulates a worst-case scenario: a complete vertebrectomy (removal of a vertebra), creating a highly unstable spine segment that the implant must stabilize.

ASTM F2706 establishes standardized mechanical test methods to evaluate the static (strength) and fatigue (long-term durability) performance test, defines in‑vitro mechanical test protocols for posterior occipital‑cervical (OC) and occipital‑cervical‑thoracic (OCT) spinal fixation assemblies under a vertebrectomy worst‑case model, aiming for relative mechanical comparison of implant designs, rather than defining pass‑fail performance thresholds. 


ASTM F2068 Fatigue test system of Femoral Prostheses Implants, Hip Implants Testing –

ASTM F2068: Standard Specification for Femoral Prostheses – Metallic Implants


ASTM F2068 covers metallic stemmed femoral prostheses used to replace the natural hip joint by means of hemi-arthroplasty or total hip surgical procedures. Prostheses for hemi-arthroplasty are intended to articulate with the natural acetabulum of the patient. Prostheses for total hip replacement are intended to articulate with prosthetic acetabular cups. Prostheses may have integral femoral heads or cones designed to accept modular heads. 

The mechanical strength (fatigue test ISO 7206-4, ISO 7206-6, shear strength test ASTM F1044, tensile test ASTM F1147, abrasion resistance test ASTM F1978), corrosion resistance, and biocompatibility of the head portions of one-piece integral implants are covered by this specification.

ASTM F1717 Spinal Implant Constructs Test –

ASTM F1717 Standard Test Methods for Spinal Implant Constructs in a Vertebrectomy Modelis a fundamental standard for evaluating the static and fatigue mechanical performance of spinal implant assemblies. Unlike ISO 12189, which focuses on a single device(an interbody cage), ASTM F1717 tests the entire posterior spinal construct—typically rods, screws, and cross-connectors—stabilizing a segment where a vertebral body has been removed (a "vertebrectomy" or "corpectomy" model). It simulates worst-case spinal instability to assess the implant's ability to maintain alignment and support loads.

ASTM F1798 Spinal Implant Subassembly Static and Fatigue Testing System –

ASTM F1798 Standard Test Method for Evaluating the Static and Fatigue Properties of Interconnection Mechanisms and Subassemblies Used in Spinal Arthrodesis Implants.

ASTM F1798 provides standardized methods for mechanically testing the interconnections within spinal implant systems. It is for evaluating the uniaxial static/fatigue strength and loosening resistance of interconnection mechanisms in spinal arthrodesis implant subassemblies, providing a standardized way to characterize mechanical performance of connections like rod-clamp, screw-rod, and hook-rod assemblies. It is critical for design validation, regulatory compliance, and clinical safety in the spinal implant industry.

ASTM F2942 Vascular Implants Axial, bending, torsional and compression durability testing –

ASTM F2942 specifies in vitro test methodologies to evaluate the cyclic durability of vascular stents under non-radial mechanical deformations (axial, bending, and torsion) that occur in vivo due to musculoskeletal motion, breathing, or cardiac activity. 

ISO 7198 Mechanical Tests and Other Evaluations for Vascular Implants –

ISO 7198 specifies test and performance requirements for tubular vascular grafts and vascular patches (surgical vascular prostheses). It defines mechanical tests (with full method/equipment/sample details) and other physicochemical, biological, dimensional, preclinical/clinical tests.

Frequently asked questions: ISO 5832 Tensile Testing for Surgical Implant Metals

1, What is ISO 5832?

ISO 5832 is the international standard series for metallic materials used in surgical implants, issued by ISO/TC 150. Each part covers one alloy — stainless steel, unalloyed titanium, titanium alloys or cobalt-based alloys — and specifies its chemical composition, microstructure, mechanical properties and test methods. It applies to raw stock such as bar, rod, wire, sheet and strip, not to finished implants.


2, Which mechanical tests does ISO 5832 require?

Room-temperature tensile testing to ISO 6892-1 is required in every part: tensile strength Rm, proof strength Rp0.2 and elongation after fracture A. Reduction of area Z is required only by ISO 5832-2 and ISO 5832-11. A bend test to ISO 7438 is required only for sheet and strip under ISO 5832-2 and ISO 5832-3. No part of ISO 5832 requires fatigue testing.


3, What tensile testing machine accuracy does ISO 5832 require?

ISO 5832 refers tensile testing to ISO 6892-1, which requires the testing machine force system to meet ISO 7500-1 class 1 as a minimum; most implant-material laboratories specify class 0.5. The extensometer must meet ISO 9513 class 1 or better for proof strength and modulus. UnitedTest machines are supplied calibrated to ISO 7500-1 class 0.5 with ISO 9513 class 0.5 extensometers.


4, What strain rate should I use for ISO 5832 tensile tests?

ISO 6892-1 Method A, the reference method, uses a strain rate of about 0.00025 s-1 up to the proof strength and no more than 0.008 s-1 in the plastic range up to tensile strength. On a 50 mm parallel length, 0.00025 s-1 is roughly 0.75 mm/min, so the machine must hold speed smoothly well below 1 mm/min. Method B stress-rate control is the permitted alternative.


5, What gauge length is specified for ISO 5832 specimens?

The proportional gauge length L0 = 5.65 × √S0, or 50 mm, where S0 is the original cross-sectional area in square millimetres. ISO 5832-2, -3, -4, -5 and -6 state this explicitly, and ISO 5832-1 and -3 additionally require the gauge length actually used to be reported together with the test result. Test software should print L0 on every report.


6, What happens if the tensile specimen breaks outside the gauge length?

ISO 5832 treats this as a separate case from an in-gauge failure. If the piece fractures outside the gauge limits, the test is acceptable if the specified requirements are met — or, in Parts 2, 5, 6, 9, 12 and 14, specifically if the elongation after fracture meets the requirement. Otherwise the test is discarded and a retest is performed.


7, How many retests are required after a failed ISO 5832 tensile test?

For each test piece that fails within the gauge limits, two retest pieces must be tested in the same manner, and the material conforms only if both retests meet the specified requirements. If any retest fails, the product is non-conforming, although the manufacturer may re-heat-treat the material and resubmit it. ISO 5832-1 and -9 route retests through ISO 404.


8, What machine capacity is needed for ISO 5832 implant materials?

Most bar and plate work is covered by a 50 kN or 100 kN frame — the strongest condition, ISO 5832-7 spring temper at 1650 MPa, needs about 130 kN on a Ø10 mm bar. Fine wire is the harder case: ISO 5832-1 covers wire down to 0.025 mm, so a 1 kN or 5 kN load cell or a dedicated low-force frame is required for those conditions.


9, Which ISO 5832 parts need a bend test, and what mandrel is used?

Only ISO 5832-2 and ISO 5832-3, and only for sheet and strip, tested to ISO 7438 by bending at least 105° around a mandrel. ISO 5832-3 uses a mandrel diameter of 10 t. ISO 5832-2 uses 3 t to 6 t depending on grade and thickness, where t is the sheet or strip thickness. A compliant lab needs an ISO 7438 bend fixture in addition to the tensile frame.


10, Is ISO 6892-1 the same as ASTM E8/E8M?

No. The two are broadly equivalent in purpose but differ in specimen dimensions, tolerances and test-speed definitions, so reports are not automatically interchangeable. Laboratories exporting to the EU test and report to ISO 6892-1; laboratories exporting to the USA use ASTM E8/E8M. UnitedTest software can report results in either format from a single test.


11, Which ASTM specification matches each ISO 5832 part?

ISO 5832-1 matches ASTM F138/F139, -2 matches ASTM F67, -3 matches ASTM F1472 (or F136 for ELI), -4 matches ASTM F75, -5 matches ASTM F90, -6 matches ASTM F562, -7 matches ASTM F1058, -8 matched ASTM F563 (now withdrawn), -9 matches ASTM F1586, -11 matches ASTM F1295 and -12 matches ASTM F1537. ISO 5832-14 has no direct ASTM counterpart.


12, Can one machine test all ISO 5832 materials?

Yes, if it is specified for the range: a class 0.5/1 frame of 50–100 kN, a changeable 1–10 kN load cell for fine wire, closed-loop strain-rate control to ISO 6892-1 Method A, an ISO 9513 class 0.5 extensometer, wedge, threaded and fine-wire grips, and an ISO 7438 bend fixture. Software must report Rm, Rp0.2, A and Z, record fracture position and print the gauge length used.


13: How UnitedTest supports customers for ISO 5832‑compliant tensile‑test workflow?

A: UnitedTest universal testing‑machine solutions include:

‑ Hardware: configurable load‑cells, clip‑on / video extensometer, interchangeable fixture kits for bar, wire, sheet‑strip for implant‑metal specimens.

‑ Software: built‑in ISO 6892‑1 calculation module, configurable gauge‑length options, fracture‑position logging, report‑template editable for ISO 5832‑series lab‑reports.

‑ Technical support: guidance for test‑setup, specimen‑gripping and applying ISO 5832 retest acceptance rules for surgical‑implant‑material QC labs & material suppliers.

< Previous: ISO 5636-5 Air Permeability test Paper and board

> Next: ISO 5840 Heart valve prostheses testing methods

Require More Customized Solutions?

We offer customization to meet your specific needs. Our expert team will collaborate with you to develop the perfect product for you
Customize Now